Polyester resin for low-cost high-hardness powder coating and preparation method of polyester resin
The polyester resin with low acid value and high functionality prepared through polymerization reaction is paired with PT910 curing agent to solve the problems of poor storage stability and low hardness of powder coatings, realize low-cost, high-hardness powder coatings, and reduce the dosage of PT910 curing agent. And improve the utilization efficiency of HAA by-products.
Patent Information
- Application Number
- CN202410999187.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing outdoor weather-resistant powder coatings have poor storage stability, low hardness and high cost, mainly due to defects in the PT910 curing agent system caused by the liquidity and high epoxy equivalent of triglycidyl trimellitate.
Using 2-methyl-2-propyl-1,3-propanediol, ethylene glycol, HAA by-product, terephthalic acid, trimellitic acid, 2-ethyl-1,3-hexanediol, 2,3 -Polymerize naphthalic anhydride and other raw materials, obtain a polyester resin with low acid value and high functionality through transesterification and polymerization reaction, and combine it with the PT910 curing agent with low functionality to prepare a low-cost and high-hardness powder coating.
The storage stability, hardness and cost of powder coatings are improved. The hardness of the coating film reaches 3H and above. The overall performance is better than that of the traditional system. At the same time, HAA by-products are effectively utilized and the dosage of PT910 curing agent is reduced.
Smart Images

Figure BDA0004961088300000021 
Figure BDA0004961088300000022 
Figure BDA0004961088300000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a polyester resin for low-cost and high-hardness powder coatings and a preparation method thereof. Background Art
[0002] Powder coatings are different from ordinary solvent-based coatings and water-based coatings. Their dispersion medium is air instead of solvent and water. They have the advantages of no solvent pollution, 100% film formation, and low energy consumption. Therefore, they are widely used in indoor and outdoor coatings. At present, outdoor weather-resistant powder coatings are mainly HAA system powder coatings and TGIC system powder coatings. The HAA curing system has small molecules escaping during the curing process, resulting in obvious pinholes in thick coatings during film curing. TGIC, also known as triglycidyl isocyanurate, is banned by the EU due to its potential allergenicity. The EU mainly uses PT910 curing agent as an outdoor weather-resistant curing agent. This product is a compound of triglycidyl trimellitate and diglycidyl terephthalate in a mass ratio of 1:3. It has a certain market, but has the following shortcomings: (1) Since triglycidyl trimellitate is liquid at room temperature, the PT910 product has a low melting point, and the powder coating prepared therefrom has poor storage stability and is prone to agglomeration or even caking when stored at room temperature. (2) Due to the high content of difunctional diglycidyl terephthalate, the hardness of the cured coating is low. Generally, the hardness of the cured coating is basically H or below, making it difficult to obtain a high-hardness coating, resulting in insufficient scratch resistance. (3) Compared with TGIC, the epoxy equivalent of PT910 is too high, basically around 150g / mol, which is much higher than the epoxy equivalent of TGIC (101g / mol), resulting in excessive use of it in powder coatings, which is 1.5 times that of TGIC curing agent, resulting in higher cost of powder coatings. How to develop low-cost, storage-stable, and high-hardness powder coatings for the PT910 curing agent system has been a research direction in the industry. Summary of the invention
[0003] In view of the above problems, the present invention provides a low-cost and high-hardness polyester resin for powder coatings, which is mainly obtained by polymerization using 2-methyl-2-propyl-1,3-propanediol, ethylene glycol, HAA byproducts, terephthalic acid, trimellitic acid, 2-ethyl-1,3-hexanediol, 2,3-naphthalic anhydride, etc. as raw materials. First, ethylene glycol and 2-methyl-2-propyl-1,3-propanediol are used to carry out an ester exchange reaction on the HAA byproduct, and the mixed polyol modified by the HAA byproduct is obtained by filter pressing, and then it is polymerized with other raw materials to finally obtain a low-acid polyester resin with higher functionality. The powder coating prepared by combining the low-acid and high-functionality polyester resin with the low-functionality PT910 curing agent has good performance and provides a way to utilize HAA byproducts with high added value.
[0004] A low-cost high-hardness polyester resin for powder coatings, comprising the following raw materials in parts by weight:
[0005]
[0006] The raw materials also include a catalyst and an antioxidant; the amount of the catalyst is 0.15-0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol; the amount of the antioxidant is 0.8-1.2% of the mass of 2-methyl-2-propyl-1,3-propanediol.
[0007] Furthermore, the HAA by-product is the by-product remaining after the crystallization mother liquor of the HAA product is distilled, and its main component is the monoamide product of dimethyl adipate and diethanolamine, which accounts for 80-85% of the mass fraction of the HAA by-product, and its molecular structure is:
[0008]
[0009] A small amount is unreacted diethanolamine, accounting for 4-8% of the mass fraction of HAA by-products; a small amount of high molecular weight polymerization product, accounting for 2-5% of the mass fraction of HAA by-products; a very small amount of HAA product, accounting for 1-3% of the mass fraction of HAA by-products; the remainder is methanol (commercially available, for example, from Anhui Huizhou Zhengjie Technology Co., Ltd.).
[0010] Preferably, the catalyst is monobutyltin oxide; and the antioxidant is antioxidant 1076.
[0011] The method for preparing the polyester resin for low-cost and high-hardness powder coating as described above comprises the following steps:
[0012] A. Add the formulated amount of 2-methyl-2-propyl-1,3-propanediol, ethylene glycol and catalyst into the transesterification reaction kettle, stir evenly, add the HAA byproduct, start the vacuum system, heat to 98-105°C and keep warm for transesterification reaction, and remove the residual methanol solvent in the HAA byproduct during the heating process;
[0013] B. Take samples for testing. When almost no methanol is evaporated during the ester exchange process, it means that the terminal methyl ester in the HAA by-product structure has been completely exchanged with 2-methyl-2-propyl-1,3-propanediol and ethylene glycol. At this time, release the vacuum system, filter the materials in the reactor through a filter while hot to remove insoluble impurities, and obtain the filtered HAA by-product modified mixed polyol;
[0014] C. Add the obtained HAA byproduct modified mixed polyol into a polymerization reactor, heat it to 130-135°C, add the formulated amount of terephthalic acid, stir it thoroughly, then gradually heat it to 190-195°C, and then carry out heat preservation polymerization reaction;
[0015] D. Take samples for testing. When the acid value of the polymer reaches 15-22 mgKOH / g, add the formulated amount of trimellitic acid and raise the temperature to 220-225°C to carry out trifunctional chain extension polymerization reaction;
[0016] E. Take samples to test the acid value of the reaction polymer. When the acid value is 36-45 mgKOH / g, add the formulated amount of 2-ethyl-1,3-hexanediol and continue the polymerization reaction at 220-225°C;
[0017] F. Take samples for testing. When the acid value of the polymer reaches 23-29 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system and raise the temperature to 230-235°C for vacuum polycondensation reaction;
[0018] G. When the acid value of the polymer drops to 8-14 mgKOH / g, release the vacuum, then add the formulated amount of 2,3-naphthalene dicarboxylic anhydride, and keep warm to carry out carboxyl end-capping reaction. When the acid value of the polymer reaches 26-31 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
[0019] Preferably, in step A, the vacuum system during the ester exchange reaction is controlled at -0.095Mpa to -0.097Mpa; in step B, the filter mesh aperture is 100-120 mesh; in step C, the temperature is gradually increased to 190-195°C at a heating rate of 14-16°C / h and then a heat preservation polymerization reaction is carried out; in step F, the vacuum degree of the vacuum system is maintained at -0.092Mpa to -0.095Mpa; in step G, the polyester resin is cooled using a steel belt with condensed water.
[0020] The obtained product is light yellow transparent particles with an acid value of 18-23 mgKOH / g and a softening point of 120-128°C.
[0021] The present invention also relates to the use of the polyester resin for low-cost and high-hardness powder coatings or the polyester resin for low-cost and high-hardness powder coatings prepared by the preparation method in a PT910 curing system.
[0022] The PT910 curing system formula includes not only the polyester resin obtained above and the PT910 curing agent, but also titanium dioxide, barium sulfate, leveling agent, brightener, benzoin, etc. The coating preparation method is as follows: according to the PT910 curing powder coating formula, the materials are mixed evenly, extruded, tableted, and crushed by a twin-screw extruder, and then the tablets are crushed and sieved to form a powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment by an electrostatic spray gun, and cured to obtain the coating.
[0023] Beneficial effects:
[0024] The low-cost and high-hardness polyester resin for powder coatings of the present invention is mainly obtained by polymerization using raw materials including 2-methyl-2-propyl-1,3-propanediol, ethylene glycol, HAA byproducts, terephthalic acid, trimellitic acid, 2-ethyl-1,3-hexanediol, 2,3-naphthalic anhydride, etc.; firstly, ethylene glycol and 2-methyl-2-propyl-1,3-propanediol are used to carry out ester exchange reaction on HAA byproducts, and the mixed polyols modified by HAA byproducts are obtained by filter pressing, and then the mixed polyols are combined with other raw materials for polymerization to finally obtain a polyester resin with a high functionality and a low acid value (18-23 mgKOH / g). The powder coating prepared by combining the low-acid value and high-functionality polyester resin with the lower-functionality PT910 curing agent has the advantages of small amount of PT910 curing agent used and low cost of powder coating, and has good storage stability. After sufficient curing, the hardness of the coating film is basically 3H or above, and the comprehensive performance is relatively good. At the same time, due to the comprehensive utilization of HAA by-products, not only the raw material cost of the polyester resin is low, but also a way is provided for the high added value utilization of HAA by-products.
[0025] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.
[0027] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.
[0028] HAA by-product is the by-product remaining after distillation of the crystallization mother liquor of HAA product. Its main component is the monoamide product of dimethyl adipate and diethanolamine, accounting for 80-85% of the mass fraction of HAA by-product. Its molecular structure is mainly:
[0029]
[0030] A small amount is unreacted diethanolamine, accounting for 4-8% of the mass fraction of HAA by-products; a small amount of high molecular weight polymerization product, accounting for 2-5% of the mass fraction of HAA by-products; a very small amount of HAA product, accounting for 1-3% of the mass fraction of HAA by-products; the remainder is methanol (commercially available, purchased from Anhui Huizhou Zhengjie Technology Co., Ltd.).
[0031] Preparation Example 1
[0032] A low-cost high-hardness polyester resin for powder coatings, comprising the following raw materials in parts by weight:
[0033]
[0034] The catalyst is monobutyltin oxide, and the amount of the catalyst is 0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol;
[0035] The antioxidant is antioxidant 1076; the amount of the antioxidant is 1% of the mass of 2-methyl-2-propyl-1,3-propanediol.
[0036] The method for preparing the polyester resin for low-cost and high-hardness powder coating comprises the following steps:
[0037] A. Add the formulated amount of 2-methyl-2-propyl-1,3-propanediol, ethylene glycol and catalyst into the transesterification reaction kettle, stir evenly, add HAA byproduct, start the vacuum system, heat to 105°C and keep warm to carry out the transesterification reaction. During the heating process, remove the residual methanol solvent in the HAA byproduct. The vacuum system during the transesterification reaction is controlled at -0.097Mpa;
[0038] B. Take samples for testing. When almost no methanol is evaporated during the ester exchange process, it indicates that the terminal methyl ester in the HAA by-product structure has been completely exchanged with 2-methyl-2-propyl-1,3-propanediol and ethylene glycol. At this time, release the vacuum system, filter the materials in the reactor while hot through a filter screen to remove insoluble impurities. The filter screen has an aperture of 100 meshes, and obtain the HAA by-product modified mixed polyol after filtration;
[0039] C. Add the obtained HAA byproduct modified mixed polyol into a polymerization reactor, heat it to 135°C, add the formulated amount of terephthalic acid, stir it thoroughly, then gradually heat it to 195°C at a heating rate of 16°C / h and then carry out heat preservation polymerization reaction;
[0040] D. Take samples for testing. When the acid value of the polymer reaches 15-22 mgKOH / g, add the formulated amount of trimellitic acid and heat to 225°C to carry out trifunctional chain extension polymerization reaction;
[0041] E. Take samples to test the acid value of the reaction polymer. When the acid value is 36-45 mgKOH / g, add the formulated amount of 2-ethyl-1,3-hexanediol and continue the polymerization reaction at 225°C;
[0042] F. Take samples for testing. When the acid value of the polymer reaches 23-29 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system, and raise the temperature to 230-235°C for vacuum polycondensation reaction. The vacuum degree is maintained at -0.095Mpa;
[0043] G. When the acid value of the polymer drops to 8-14 mgKOH / g, release the vacuum, then add the formulated amount of 2,3-naphthalene dicarboxylic anhydride, and keep warm to carry out carboxyl end-capping reaction. When the acid value of the polymer reaches 18-23 mgKOH / g, stop the reaction, discharge the material while hot, and cool the polyester resin with a steel belt with condensed water, then crush and granulate it to obtain polyester resin.
[0044] The obtained product is light yellow transparent particles with an acid value of 19 mgKOH / g and a softening point of 127°C.
[0045] Preparation Example 2
[0046] A low-cost high-hardness polyester resin for powder coatings, comprising the following raw materials in parts by weight:
[0047]
[0048] The catalyst is monobutyltin oxide; the amount of the catalyst is 0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol;
[0049] The antioxidant is antioxidant 1076; the amount of the antioxidant is 1.2% of the mass of 2-methyl-2-propyl-1,3-propanediol.
[0050] The preparation method is the same as Example 1.
[0051] The obtained product is light yellow transparent particles with an acid value of 21 mgKOH / g and a softening point of 124°C.
[0052] Preparation Example 3
[0053] A low-cost high-hardness polyester resin for powder coatings, comprising the following raw materials in parts by weight:
[0054]
[0055] The catalyst is monobutyltin oxide; the amount of the catalyst is 0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol;
[0056] The antioxidant is antioxidant 1076; the amount of the antioxidant is 1% of the mass of 2-methyl-2-propyl-1,3-propanediol.
[0057] The preparation method is the same as that of Example 1.
[0058] The obtained product is light yellow transparent particles with an acid value of 20 mgKOH / g and a softening point of 126°C.
[0059] Preparation Example 4
[0060] A low-cost high-hardness polyester resin for powder coatings, comprising the following raw materials in parts by weight:
[0061]
[0062] The catalyst is monobutyltin oxide; the amount of the catalyst is 0.15-0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol;
[0063] The antioxidant is antioxidant 1076; the amount of the antioxidant is 0.8-1.2% of the mass of 2-methyl-2-propyl-1,3-propanediol.
[0064] The preparation method is the same as Example 1.
[0065] The obtained product is light yellow transparent particles with an acid value of 22 mgKOH / g and a softening point of 121°C.
[0066] Comparative Preparation Example 1
[0067] Commercially available ordinary polyester resin, with an acid value of 35 mgKOH / g, a softening point of 110°C, model SJ4A, was purchased from Anhui Shenjian New Materials Co., Ltd.
[0068] Comparative Preparation Example 2
[0069] The raw materials are the same as those in Comparative Example 1, except that the amount of PT910 curing agent in the following PT910 curing powder coating system formula is increased from 30 parts to 50 parts, and the mass parts of other raw materials remain unchanged.
[0070] Examples 1-4 and Comparative Examples 1 and 2 (polyester resins are obtained by the above-mentioned preparation examples or comparative preparation examples, respectively)
[0071] According to the powder coating formula of PT910 curing agent, the formula in parts by weight is as follows:
[0072]
[0073] Preparation of coating: Mix all materials according to the formula of PT910 curing powder coating, extrude, tablet and crush with a twin-screw extruder, and then crush and sieve the flakes to make powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment with an electrostatic spray gun, and cured at 200℃ / 12min to obtain the coating.
[0074] Performance comparison
[0075] Coating index testing is based on: GB / T 21776-2008 "Testing Standard Guide for Powder Coatings and Their Coatings". The pencil hardness parameters are 3B-2B-B-HB-FH-2H-3H-4H, and the hardness level increases gradually from left to right.
[0076] The polyester resins prepared in the above examples and comparative examples were used to prepare coatings according to the coating formulations provided by the present invention, and the coating properties were tested as shown in Tables 1 and 2 below.
[0077] Table 1 Coating properties of powder coatings
[0078]
[0079] Table 2 Storage stability of powder coatings
[0080] sample Storage stability (45℃ / 100 days) Storage stability (45℃ / 200 days) Example 1 Uniform and loose Uniform and loose Example 2 Uniform and loose Uniform and loose Example 3 Uniform and loose Uniform and loose Example 4 Uniform and loose Uniform and loose Comparative Example 1 Very little agglomeration A small amount of clumping Comparative Example 2 A small amount of clumping Obvious clumping
[0081] As can be seen from Table 1, the powder coating prepared by combining the polyester resin prepared by the product of the present invention with the PT910 curing agent is uniformly dispersed, can be fully cured at 200℃ / 12min, the coating appearance is flat and smooth after curing, and both positive and negative impacts of 50cm are passed. The gloss of the coating is basically above 93%, and there is no obvious change after boiling in boiling water for 2h. At the same time, the hardness of the cured coating can reach 3H, which has a better coating hardness. However, due to the high acid value of the polyester resin and the insufficient amount of PT910 curing agent in Comparative Example 1, effective curing cannot be achieved, and the impact resistance, gloss and hardness are all poor; while Comparative Example 2 can achieve full curing after increasing the amount of PT910 curing agent to 55 parts, and the coating appearance is flat and smooth, the 50cm impact resistance is passed, and the gloss is also good, but the coating hardness is average, and the hardness can only reach H. In terms of storage stability of the powder coating, as shown in Table 2, the product of the present invention has good storage stability at 45°C, and is in a uniformly dispersed state at 45°C for 100 days and 200 days, with almost no agglomeration. In Comparative Example 1, the powder coating has very little agglomeration at 45°C / 100 days, and a small amount of agglomeration at 45°C / 200 days; and in Comparative Example 2, due to the obvious increase in the amount of PT910 curing agent, the powder coating has obvious agglomeration, with a small amount of agglomeration at 45°C / 100 days and obvious agglomeration at 45°C / 200 days, which is significantly worse than the product of the present invention.
[0082] The product of the present invention not only develops a low-cost, low-acid value, high-hardness polyester resin suitable for PT910 curing agent, but also has low cost of polyester resin and reduces the amount of PT910 used in the powder coating formula, further reducing the cost of powder coating. Moreover, more HAA by-products are used in the synthesis process, providing a new way for the comprehensive utilization of HAA by-products.
[0083] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.
Claims
1. A low-cost high-hardness polyester resin for powder coating, characterized in that: The invention comprises the following raw materials in parts by weight: The raw materials also include a catalyst and an antioxidant; the amount of the catalyst is 0.15-0.2% of the mass of 2-methyl-2-propyl-1,3-propanediol; the amount of the antioxidant is 0.8-1.2% of the mass of 2-methyl-2-propyl-1,3-propanediol.
2. A low-cost, high-hardness polyester resin for powder coatings as claimed in claim 1, further characterized in that the HAA by-product is a by-product remaining after distillation of the crystallization mother liquor of the HAA product, and the main component is a monoamide product of dimethyl adipate and diethanolamine, accounting for 80-85% of the mass fraction of the HAA by-product, and its molecular structure is:
3. A polyester resin for low-cost and high-hardness powder coating as claimed in claim 1, further characterized in that the catalyst is monobutyl tin oxide.
4. A low-cost, high-hardness polyester resin for powder coating as claimed in claim 1, further characterized in that the antioxidant is antioxidant 1076.
5. The method for preparing a low-cost high-hardness polyester resin for powder coatings according to any one of claims 1 to 4, characterized in that: The following steps are involved: A. Add the formulated amount of 2-methyl-2-propyl-1,3-propanediol, ethylene glycol and catalyst into the transesterification reaction kettle, stir evenly, add the HAA byproduct, start the vacuum system, heat to 98-105°C and keep warm for transesterification reaction, and remove the residual methanol solvent in the HAA byproduct during the heating process; B. Take samples for testing. When almost no methanol is evaporated during the ester exchange process, it means that the terminal methyl ester in the HAA by-product structure has been completely exchanged with 2-methyl-2-propyl-1,3-propanediol and ethylene glycol. At this time, release the vacuum system, filter the materials in the reactor through a filter while hot to remove insoluble impurities, and obtain the filtered HAA by-product modified mixed polyol; C. Add the obtained HAA byproduct modified mixed polyol into a polymerization reactor, heat it to 130-135°C, add the formulated amount of terephthalic acid, stir it thoroughly, then gradually heat it to 190-195°C, and then carry out heat preservation polymerization reaction; D. Take samples for testing. When the acid value of the polymer reaches 15-22 mgKOH / g, add the formulated amount of trimellitic acid and raise the temperature to 220-225°C to carry out trifunctional chain extension polymerization reaction; E. Take samples to test the acid value of the reaction polymer. When the acid value is 36-45 mgKOH / g, add the formulated amount of 2-ethyl-1,3-hexanediol and continue the polymerization reaction at 220-225°C; F. Take samples for testing. When the acid value of the polymer reaches 23-29 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system and raise the temperature to 230-235°C for vacuum polycondensation reaction; G. When the acid value of the polymer is reduced to 8-14 mgKOH / g, release the vacuum, then add the formulated amount of 2,3-naphthalene dicarboxylic anhydride, and keep warm to carry out carboxyl end-capping reaction. When the acid value of the polymer is 18-23 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.
6. The method for preparing a low-cost high-hardness polyester resin for powder coatings according to claim 5, characterized in that: In step A, the vacuum system during the transesterification reaction is controlled at -0.095 MPa to -0.097 MPa.
7. The method for preparing a low-cost high-hardness polyester resin for powder coatings according to claim 5, characterized in that: In step B, the filter screen has an aperture of 100-120 meshes.
8. The method for preparing a low-cost high-hardness polyester resin for powder coatings according to claim 5, characterized in that: In step C, the temperature is gradually increased to 190-195° C. at a heating rate of 14-16° C. / h, and then a heat preservation polymerization reaction is carried out.
9. The method for preparing a low-cost high-hardness polyester resin for powder coatings according to claim 5, characterized in that: In step F, the vacuum degree of the vacuum system is maintained at -0.092 MPa to -0.095 MPa; in step G, the polyester resin is cooled by a steel belt with condensed water.
10. Use of the low-cost high-hardness polyester resin for powder coatings according to any one of claims 1 to 4 or the low-cost high-hardness polyester resin for powder coatings prepared by the preparation method according to any one of claims 5 to 9 in a PT910 curing system.
Citation Information
Patent Citations
Saturated carboxyl polyester resin with low acid value for powder coating and synthetic method thereof
CN101560291A
Powder paint with high surface harness and decoration
CN101942262A
Polyester resin for a high-leveling self-cured powder coating and two-kettle-combined preparation method of polyester resin
CN110591066A
Liquid polyol for polyurethane adhesive, and preparation method thereof
CN112851921A
Mixed 50 / 50 low-cost high-hardness polyester resin for powder coating and preparation method
CN114181385A