Two-component coating composition, preparation method thereof and coated product

Through the use of the two-component coating composition, the problems of complicated construction and poor performance of the existing anti-corrosion coating system are solved, and a coating with simple construction, environmental protection and excellent performance is realized, which is suitable for a wide range of applications.

CN118725708APending Publication Date: 2024-10-01VALSPAR COATINGS(SHANGHAI) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310334627.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing anti-corrosion coating system has complex construction and high cost, and the coating performance of water-based anti-corrosion coating is poor, making it difficult to meet environmental protection and performance requirements.

Method used

A two-component coating composition is used, in which component A contains a hydroxyl-functional polyurethane dispersion and anti-rust pigment, and component B contains a non-hydrophilic isocyanate curing agent. It is prepared by simple mixing to form a product with excellent salt spray resistance, weather resistance, Mechanical properties and adhesion of the coating.

Benefits of technology

It has achieved a simple and environmentally friendly anti-corrosion coating with high salt spray resistance, weather resistance, mechanical properties and adhesion, as well as low VOC and low cost, making it suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004156795890000071
    Figure BDA0004156795890000071
  • Figure BDA0004156795890000101
    Figure BDA0004156795890000101
  • Figure BDA0004156795890000191
    Figure BDA0004156795890000191
Patent Text Reader

Abstract

The invention relates to a two-component coating composition, a preparation method thereof and a coated product. The two-component coating composition comprises a component A and a component B. The two-component coating composition is characterized in that the component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, the component B comprises a non-hydrophilic isocyanate curing agent, the fineness change rate of the component A relative to the initial fineness after 14 days at 40 DEG C is 10% or lower, and the fineness change rate of the component B relative to the initial fineness after 14 days at 40 DEG C is 10% or lower. And the fineness is measured by using a fineness plate according to GB / T 1724-2019. The two-component coating composition provided by the invention can provide a coating with excellent salt mist resistance, weather resistance, mechanical property, adhesive force and chemical resistance, and has the characteristics that the primer and the finish are integrated, the construction is simple, and the environment is protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal surface corrosion protection, and in particular to a two-component coating composition, a preparation method thereof, and a coated product. Background Art

[0002] With the rapid development of economy, coatings applied to metal substrates face more and more problems and higher and higher requirements.

[0003] For example, most of the existing anti-corrosion coating systems use a primer, an intermediate paint, a topcoat, or a composite anti-corrosion coating system of a primer and a topcoat. This system has the disadvantages of a long construction period and high construction cost due to its complicated operation process.

[0004] Moreover, a relatively large amount of organic solvents are mostly used in traditional anti-corrosion coating systems. As people pay more and more attention to environmental issues, the laws and regulations of various countries and regions on environmental protection issues are becoming more and more stringent, and it is becoming more and more important to reduce the amount of organic solvents in the coating system. The water-based anti-corrosion system proposed by some researchers involves a modified hydrophilic curing agent. However, this modified hydrophilic curing agent usually involves complex synthesis processes and raw materials, which greatly increases the cost of the coating and affects the promotion and application of water-based coatings. Moreover, the coatings formed by existing water-based anti-corrosion coatings usually show poor coating properties, such as reduced gloss, insufficient salt spray resistance, etc., and therefore still cannot meet people's requirements. Summary of the invention

[0005] In view of this, there is a need for an anticorrosive coating system that has good construction performance and satisfactory environmental performance, and can provide excellent coating performance. More specifically, there is a need for a coating system that is simple to construct, green and environmentally friendly, and can provide an anticorrosive coating with excellent salt spray resistance, weather resistance, mechanical properties, adhesion, and chemical resistance.

[0006] The above objectives are achieved by the two-component coating composition described herein.

[0007] The first aspect of the present application provides a two-component coating composition, comprising component A and component B, characterized in that component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, component B comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of component A relative to the initial fineness after 14 days at 40°C is 10% or less, and the fineness is measured using a fineness plate in accordance with GB / T 1724-2019.

[0008] The second aspect of the present application provides a method for preparing a two-component coating composition, comprising mixing component A and component B, characterized in that component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, component B comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of component A relative to the initial fineness after 14 days at 40°C is 10% or less, and the fineness is measured using a fineness plate in accordance with GB / T 1724-2019.

[0009] The third aspect of the present application provides a coated product, characterized in that the coated product comprises: a metallic substrate having at least one main surface; and a two-component coating composition described herein or a cured coating thereof coated on the at least one main surface of the metallic substrate.

[0010] The inventors surprisingly found that the two-component coating composition described in the present application has the advantages of simple construction and green environmental protection, and can provide a coating system of an anti-corrosion coating with excellent properties (e.g., salt spray resistance, weather resistance, mechanical properties, adhesion and chemical resistance). In particular, the coating or cured paint film of the present application has one or more of the following characteristics: no blistering for at least 1000 hours in a neutral salt spray test on an aluminum plate, a phosphated plate or both at 35°C, no blistering for at least 120 hours in a 5% sulfuric acid solution at 20°C, no blistering for at least 120 hours in a 5% sodium hydroxide solution at 20°C, and no blistering after exposure to a xenon lamp for 1000 hours with a ΔE of no more than 1.0 and a gloss retention rate of more than 80% at 60°.

[0011] Moreover, the two-component coating composition of the present application has the advantages of low VOC (the amount of organic solvent does not exceed 15% of the total weight of the composition, or is even solvent-free) and low cost. It is a healthy and environmentally friendly product and is more easily accepted and promoted by consumers.

[0012] The above summary of the present application is not intended to describe each disclosed embodiment or every implementation of the present application. Illustrative embodiments are more particularly exemplified in the following description. DETAILED DESCRIPTION

[0013] definition

[0014] As used herein, "a", "an", "the", "at least one" and "one or more" and the absence of quantifiers may be used interchangeably unless otherwise indicated. Thus, for example, a coating composition comprising "an" additive may be interpreted to mean that the coating composition comprises "one or more" additives. Unless otherwise indicated herein, the use of the singular form herein is intended to include the plural form.

[0015] Unless otherwise expressly stated, the use of the terms "includes," "comprising," "containing," and "having" should generally be interpreted as open-ended and non-restrictive. For example, where a composition is described as including or comprising specific components, it is expected that optional components not mentioned in the present application are not excluded from the composition, and it is expected that the composition can be composed of or consist of the mentioned components, or where a method is described as including or comprising specific process steps, it is expected that optional process steps not mentioned in the present application are not excluded from the method, and it is expected that the method can be composed of or consist of the mentioned process steps.

[0016] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0017] Unless otherwise indicated, the term "consisting essentially of..." means that in addition to the described elements, the subject (e.g., composition, method, or structure) may include additional elements (e.g., ingredients, steps, and / or parts), but the additional elements (e.g., ingredients, steps, and / or parts) do not substantially change the basic and novel characteristics of the subject (e.g., composition, method, or structure). Therefore, depending on the circumstances, the term "consisting essentially of..." preferably means that the majority (e.g., 90% or more, such as 95% or more, particularly 99% or more, even more particularly 99.5% or more) of the subject consists of the described elements, including being completely composed of the described elements (i.e., 100%).

[0018] Unless otherwise indicated, each point or single value between the endpoints of a range is included in the range. For example, a range of 1 to 5 includes the values ​​1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc. Moreover, a disclosed numerical range includes all subset ranges within the broader range, for example, a range of 1 to 5 includes subranges 1 to 4, 1.5 to 4.5, 1 to 2, etc. Thus, each point or single value can be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits, and the resulting range belongs to the content explicitly disclosed in this application.

[0019] As used herein, the term "or" is inclusive. That is, the phrase "A or (or) B" means "A, B, or both A and B", which may also be abbreviated as "A and / or B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist). In contrast, the exclusive "or (or)" is represented herein, for example, by terms such as "either A or B" and "one of A or B".

[0020] When used in the context of a "coating applied to a surface or substrate," the term "on" includes coatings applied directly or indirectly to a surface or substrate. Thus, for example, a coating applied to a primer layer on a substrate is counted as a coating applied to the substrate.

[0021] The term "anticorrosive coating composition" refers to a coating composition which, when applied in one or more layers to a metallic substrate, forms a coating that can be exposed to corrosive conditions for a considerable period of time (e.g., salt spray exposure for three weeks, five weeks or more) without causing objectionable visible deterioration or corrosion or swelling.

[0022] As used herein, the term "hydroxy functional" means containing at least one unreacted hydroxy functional group.

[0023] When used in this article, the terms "hydrophilic curing agent" and "non-hydrophilic curing agent" have meanings known in the art. Generally, non-hydrophilic curing agents (also referred to as hydrophobic curing agents or oily curing agents) are difficult to mix evenly with water or aqueous A component, and phase separation is easily caused. For example, non-hydrophilic curing agents include most unmodified polyisocyanates. Hydrophilic curing agents are usually obtained by hydrophilically modifying curing agents. Hydrophilic curing agents can be, for example, non-ionic hydrophilic modified (e.g., Bayhydur series of Covestro), ionic modified, non-ionic and ionic composite modified.

[0024] The terms "preferred" and "preferably" refer to embodiments of the present application that may provide certain benefits in certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. In addition, the description of one or more preferred embodiments does not mean that other embodiments are not applicable, and is not intended to exclude other embodiments from the scope of the present application.

[0025] Unless otherwise specified, the methods or processes described herein are carried out under standard environmental conditions known in the art, for example, at 25° C., 101325 Pa and 40% to 80% (eg, 50% or 60%) relative humidity (RH).

[0026] Two-component coating composition

[0027] The two-component coating composition according to the first aspect of the present application comprises component A and component B, wherein component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, component B comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of component A relative to the initial fineness after 14 days at 40°C is 10% or less, and the fineness is measured using a fineness plate according to GB / T 1724-2019.

[0028] After in-depth research and screening, the inventors surprisingly found that the fineness change rate of component A containing anti-rust pigments has a significant effect on the performance of the coating composition. In this article, the inventors use appropriate conditions to determine the fineness change rate. The test conditions described in this article can accurately characterize the fineness change rate, and can not take too long while keeping the coating system basically stable, so that the test process can be conveniently and easily carried out in actual industrial applications. The fineness change rate relative to the initial fineness after 14 days at 40°C can determine the ionic stability of the anti-rust pigment. A lower fineness change rate is desired. In some embodiments, the fineness change rate can be about 9% or less, preferably about 8% or less, more preferably about 7% or less, and even more preferably about 6% or less. For example, the fineness change rate can be about 5% or less, about 4% or less, about 3% or less, about 2% or less, or about 1% or less.

[0029] Hydroxy-functional polyurethane dispersion preferably has higher hydroxyl value.In some embodiments, the hydroxyl value of hydroxyl-functional polyurethane dispersion can be about 40-200mg KOH / g, preferably about 60-150mg KOH / g, more preferably about 80-120mg KOH / g.For example, the hydroxyl value of hydroxyl-functional polyurethane dispersion can be about 60mg KOH / g, about 70mg KOH / g, about 80mg KOH / g, about 90mg KOH / g, about 100mg KOH / g, about 110mg KOH / g, about 120mg KOH / g, about 130mg KOH / g, about 140mg KOH / g, about 150mg KOH / g or about 180mg KOH / g.

[0030] The minimum film-forming temperature of the hydroxyl-functional polyurethane dispersion is preferably ≥ 16° C., more preferably 18-60° C., even more preferably 25-50° C. For example, the minimum film-forming temperature of the hydroxyl-functional polyurethane dispersion is about 20° C., about 30° C., about 35° C., about 40° C., or about 45° C.

[0031] In some embodiments, the Brookfield viscosity of the hydroxy-functional polyurethane dispersion at 25°C is 500-5000 mPa·s. The Brookfield viscosity of the hydroxy-functional polyurethane dispersion at 25°C is preferably 800 mPa·s or higher, or 4800 mPa·s or lower. For example, the Brookfield viscosity of the hydroxy-functional polyurethane dispersion at 25°C may be 1000 mPa·s, 1500 mPa·s, 2000 mPa·s, 2500 mPa·s, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s or 4500 mPa·s. The Brookfield viscosity may be measured using known instruments by methods known in the art. For example, the Brookfield viscosity may be measured at 25°C using a Brookfield LV, 61#, 30 rpm according to GB / T2794-2013 or DIN 53019.

[0032] In some embodiments, the average particle size of the hydroxyl-functional polyurethane dispersion is 10-80nm. Preferably, the average particle size of the hydroxyl-functional polyurethane dispersion is about 20nm-70nm, more preferably about 25nm-60nm. For example, the average particle size of the hydroxyl-functional polyurethane dispersion is about 20nm, about 30nm, about 40nm, about 50nm, about 60nm or about 70nm. The average particle size can be determined by methods known in the art using known instruments. For example, laser correlation spectroscopy (LKS) can be used to determine the average particle size.

[0033] In some embodiments, the non-volatile content of the hydroxyl-functional polyurethane dispersion used to formulate the A component is about 20%-60%, preferably about 30-50%. For example, the non-volatile content of the hydroxyl-functional polyurethane dispersion used to formulate the A component can be about 25%, 30%, 35%, 40%, 45% or 50%.

[0034] In some embodiments, the amount of the hydroxyl-functional polyurethane dispersion is 40-80 wt %, preferably 45-75 wt %, and more preferably 50-70 wt %, based on the total weight of component A. For example, the amount of the hydroxyl-functional polyurethane dispersion can be 50 wt %, 55 wt %, 60 wt %, 65 wt %, or 70 wt %, based on the total weight of component A.

[0035] Preferably, the hydroxyl-functional polyurethane dispersion in the present application is obtained by reacting a compound with a hydroxyl-functional group with a compound with an NCO-functional group. Suitable hydroxyl-functional polyurethane resins that can be used are prepared, for example, by reacting a compound reactive for isocyanate groups with a polyisocyanate having at least 2 free isocyanate groups per molecule. High molecular weight polyols can be used as reactive compounds for isocyanate groups. Examples of polyols can include polyester polyols, polyether polyols, polycarbonate polyols, and polyurethane polyols. Preferably, polyester polyols, polyether polyols, polycarbonate polyols, or any combination thereof with a molecular weight of, for example, 500g / mol-6000g / mol are used. Examples of useful polyisocyanates include p-phenylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate. In the reaction mixture, the molar equivalent ratio of NCO / OH functional groups may be 0.2:1 to 5:1.

[0036] Preferably, the hydroxyl functional polyurethane dispersion in the present application has a narrower molecular weight distribution. In some embodiments, the hydroxyl functional polyurethane dispersion can have an average particle size of about 10nm-80nm, preferably about 15nm-70nm, and more preferably an average particle size of 20nm-50nm. For example, the hydroxyl functional polyurethane dispersion can have an average particle size of about 25nm, 30nm, 35nm, 40nm or 45nm.

[0037] Just for ease of understanding, some preferred hydroxyl-functional polyurethane dispersions in this application can be briefly represented by the following formula (a). As can be seen from formula (a), in these preferred hydroxyl-functional polyurethane dispersions, the hydroxyl groups are basically located at the ends of the segments. This is different from other hydroxyl-functional resins in the art where the hydroxyl groups are located in the side chains of the segments (for example, as shown by the following formula (b)).

[0038]

[0039] Furthermore, in the hydroxyl functional polyurethane dispersions described herein, the hydroxyl groups preferably comprise primary hydroxyl groups, more preferably consist essentially of primary hydroxyl groups. In some exemplary embodiments, 90% or more of the hydroxyl groups in the hydroxyl functional polyurethane dispersion are primary hydroxyl groups.

[0040] The inventors have found that the terminal hydroxyl functional polyurethane aqueous dispersion has the advantages of adjustable soft and hard segment ratio, easy molecular structure design, and good compatibility with non-hydrophilic isocyanate curing agent, and its coating film has excellent appearance and mechanical properties. In particular, the inventors have found that the fineness change rate of the obtained A component is very low by combining the terminal hydroxyl functional polyurethane aqueous dispersion described herein with an anti-rust pigment (especially the anti-rust pigment described herein). The inventors have also surprisingly found that the A component described herein with a very low fineness change rate can make the obtained cured coating have improved salt spray resistance, weather resistance and chemical resistance, while maintaining excellent mechanical properties and adhesion.

[0041] In some embodiments, the hydroxyl-functional polyurethane dispersion can be a polyester polyurethane dispersion. Examples of hydroxyl-functional polyurethane dispersions include, but are not limited to, Covestro Bayhydrol U XP 2755. The hydroxyl-functional polyester polyurethane dispersion described herein has improved hydrolysis resistance, good mechanical properties and placement stability, and can be applied to complex outdoor environments (humidity, high temperature, salt spray, etc.).

[0042] In some embodiments, the amount of the anti-rust pigment is 2 wt%-20 wt%, preferably 5-15 wt%, more preferably 5-10 wt%, based on the total weight of component A. For example, based on the total weight of component A, the amount of the anti-rust pigment is 3 wt%, 4 wt%, 6 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, or 20 wt%.

[0043] In some embodiments, the anti-rust pigment is or comprises calcium ion-exchanged silica. The calcium content in the anti-rust pigment is 0.5 wt %-15 wt %, preferably 1 wt %-12 wt %, more preferably 3 wt %-10 wt %. For example, the calcium content in the anti-rust pigment is 2 wt %, 4 wt %, 6 wt % or 8 wt % on a dry basis.

[0044] In some embodiments, the rust-proof pigment itself (preferably, calcium ion-exchanged silica itself) does not release or hardly releases Zn during acid washing or water washing for 1 hour. After the rust-proof pigment is acid washed or water washed for 1 hour, the Zn element cannot be detected by ICP-OES in the obtained liquid. For example, after the rust-proof pigment is acid washed and water washed for 1 hour, the Zn concentration in the obtained liquid does not exceed 10.0 mg / kg. Preferably, after the rust-proof pigment is water washed for 1 hour, the Zn element cannot be detected by ICP-OES in the obtained liquid. Preferably, after the rust-proof pigment is water washed for 1 hour, the Zn element cannot be detected by ICP-OES in the obtained liquid.

[0045] In some embodiments, the concentration of Ca in the liquid obtained by washing the antirust pigment itself (preferably, the calcium ion-exchanged silica itself) for 1 hour is no more than about 1600 mg / kg, more preferably no more than about 1000 mg / kg, and even more preferably no more than about 800 mg / kg. Preferably, the concentration of Ca in the liquid obtained by washing the calcium ion-exchanged silica itself for 1 hour is about 50 mg / kg-700 mg / kg. For example, the concentration of Ca in the liquid obtained by washing the antirust pigment itself (preferably, the calcium ion-exchanged silica itself) for 1 hour is about 700 mg / kg, about 600 mg / kg, about 500 mg / kg, about 400 mg / kg, about 300 mg / kg, about 200 mg / kg, about 100 mg / kg or about 50 mg / kg.

[0046] You can refer to GB / T 23991-2009 "Determination of soluble harmful elements in coatings". Use 0.07 mol / L hydrochloric acid solution and DI water (deionized water) respectively, extract in a constant temperature water bath oscillating tank at 37°C for 1 hour, filter to obtain a clear liquid, and use ICP-OES to analyze the elements (such as Zn, Ca) in the clear liquid.

[0047] In some embodiments, the oil absorption of the rust-proof pigment (preferably, the calcium ion-exchanged silica itself) is 20-100 g / 100 g. Preferably, the oil absorption of the rust-proof pigment is 90 g / 100 g or less, more preferably 80 g / 100 g or less. For example, the oil absorption of the rust-proof pigment (preferably, the calcium ion-exchanged silica itself) is 20 g / 100 g, 30 g / 100 g, 40 g / 100 g, 50 g / 100 g, 60 g / 100 g, 70 g / 100 g, 80 g / 100 g or 90 g / 100 g. The oil absorption of the rust-proof pigment can be determined by methods known in the art, for example, according to DIN ISO 787-5.

[0048] In some embodiments, the particle size of the anti-rust pigment (preferably, calcium ion exchanged silica itself) is 1.8-20 μm. Preferably 2.5-6 μm, more preferably 2.7-5 μm. For example, the particle size of the anti-rust pigment is about 2.3 μm, 2.6 μm, 3.0 μm, 3.5 μm, 4 μm or 4.5 μm. The particle size of the anti-rust pigment can be measured using a Malvern 3000E laser particle size analyzer.

[0049] In some embodiments, the pH of the anti-rust pigment (preferably, the calcium ion exchanged silica itself) is 7-10, preferably 8.0-10, more preferably 8.5-10.0. For example, the pH of the anti-rust pigment is about 8.5, 8.8, 9, 9.3, 9.5 or 9.8. The pH of the anti-rust pigment can be determined in a 10 wt% aqueous suspension. The pH of the anti-rust pigment can be determined by methods known in the art, for example, according to DIN EN ISO 787-9.

[0050] The inventor found that traditional anti-rust pigments generally use substances with strong toxicity (such as red lead, lead powder, chromate, etc.), which not only pollute the environment, but also endanger human health. Some anti-rust products use zinc-rich primers, phosphate anti-rust pigments, chromate anti-rust pigments, borate anti-rust pigments, etc. However, the content of zinc powder in zinc-rich primers is usually high, up to 85% or 95%, so the paint film of zinc-rich paint will have a large amount of zinc overflow during electric welding and cutting flame operations, and the generated steam brings serious harm to the health of operators, and operators are prone to hot zinc disease. Most of phosphate, chromate and borate anti-rust pigments are insoluble, and the dispersibility in water-based coatings is poor, resulting in the anti-rust performance of these anti-rust pigments when used alone is still not good enough. The inventor found that calcium ion exchange silica has the advantages of being free of heavy metals, non-toxic and pollution-free, and having good stability. Without wishing to be limited by theory, calcium ion exchange silica can promote the formation of chemically stable insoluble silicates in the coating system, and these insoluble silicates can migrate to the metal surface to form a passivation layer, thereby preventing electrochemical reactions on the metal surface and inhibiting the corrosion process of the metal.

[0051] In addition to calcium ion exchange silica, component A may also include other anti-rust pigments. In some embodiments, component A comprises one or more of wollastonite, strontium phosphate, zinc phosphate and zinc oxide. The inventors were surprised to find that by using a combination of specific anti-rust pigments, the salt spray resistance, acid resistance and weather resistance of the coating can be significantly improved. The combination of one or more of wollastonite, strontium phosphate, zinc phosphate and zinc oxide with calcium ion exchange silica produces a synergistic effect, and the coating performance obtained is significantly better than using a certain anti-rust pigment alone. It is not expected to be limited by theory. Calcium ion exchange silica can not only promote the generation of insoluble silicates with stable chemical properties, but also can be combined with metal oxide films to form a composite protective layer, quickly solve the salt spray problem, no blistering, high weather resistance, and improve the hardness of the paint film. In particular, the inventors found that the synergistic effect of wollastonite and calcium ion exchange silica is significantly enhanced. In some preferred embodiments, component A comprises 2% to 20% by weight of calcium ion exchange silica and 3% to 20% by weight of wollastonite. More preferably, the A component comprises 4 wt% to 10 wt% of calcium ion-exchanged silica and 4 wt% to 8 wt% of wollastonite.

[0052] The two-component coating composition, preferably component A, may also contain a silane coupling agent. In some embodiments, the coupling agent includes a silane compound having the following formula I:

[0053]

[0054] Each X 1 Independently selected from -Cl, -OCH 3 、-OCH 2 CH 3 、-OC 2 H 4 OCH 3 、-OSi(CH 3 ) 3 and-OCOCH 3 a group of persons; and

[0055] Y 1 For -Cl, -NH 2 , -SH, -OH, epoxy, -N 3 , γ-methacryloxypropyl or isocyanate-terminated alkyl.

[0056] In some embodiments, the molecular weight of the silane coupling agent is 100-800 Daltons, preferably 200-400 Daltons, such as about 150 Daltons, about 250 Daltons, 300 Daltons.

[0057] Preferably, the silane coupling agent is an epoxy silane coupling agent. For example, in Formula I, Y 1 It is an alkyl group terminated by an epoxy group.

[0058] The inventors found that, on the one hand, the active groups of the silane coupling agent react with the metal oxide or water on the metal surface to form hydrogen bonds, thereby improving the adhesion of the coating to the metal substrate; on the other hand, the silane coupling agent can further promote the effect of the anti-rust pigment in the coating composition and improve the salt spray resistance and acid resistance of the coating. In particular, when epoxy silane coupling agents are used, the benefits of these two aspects are more prominent.

[0059] More importantly, in some embodiments, by adding a relatively small amount of silane coupling agent, the beneficial effects described above can be observed. Based on the total weight of component A, the amount of the silane coupling agent can be 0.2-2 wt%, preferably 0.3-1.8 wt%, and more preferably 0.5-1.5 wt%. For example, the amount of the silane coupling agent can be about 0.4 wt%, about 0.5 wt%, about 0.6 wt%, about 0.8 wt%, about 1.0 wt%, about 1.2 wt%.

[0060] In the two-component coating composition according to the present application, the A component may also include an auxiliary agent. These auxiliary agents will not adversely affect the two-component coating composition or the cured coating obtained therefrom. Suitable auxiliary agents include, for example, those reagents that will improve the processing performance or manufacturing performance of the composition, enhance the aesthetic feeling of the composition, improve the coating composition or the specific functional properties or characteristics (such as adhesion to the substrate) of the cured composition obtained therefrom, or reduce costs. The auxiliary agent that may be included is, for example, a pigment, a lubricant, a film-forming aid, a wetting agent, a plasticizer, a defoamer, a colorant, an antioxidant, a flow control agent, a thixotropic agent, a matte powder, a dispersant, an adhesion promoter, a thickener, a pH regulator, a light stabilizer, an anti-flash rust agent, a curing accelerator, or a combination thereof. The content of each optional component is sufficient to achieve its intended purpose, but preferably, such a content will not adversely affect the two-component coating composition or the cured coating obtained therefrom. In some preferred embodiments, the A component may include a defoamer, a dispersant, a leveling agent, a light stabilizer, an anti-flash rust agent, a thickener, or any combination thereof as a conventional auxiliary agent. According to the present application, the total amount of conventional auxiliary agents is 0.3 wt % to 20 wt %, preferably 0.5-18 wt %, for example about 10 wt %, relative to the total weight of component A. In some embodiments, the amount of dispersant can be 0.1-2 wt %, the amount of defoamer can be 0.1-0.8 wt %, the amount of leveling agent can be 0.1-2 wt %, the amount of light stabilizer can be 0.5-3 wt %, and / or the amount of anti-flash rust agent can be 0.1-1 wt %.

[0061] Examples of the light stabilizer may include, but are not limited to, hindered amine compounds, hindered phenol compounds; CHIMASORB 944, TINUVIN 144, TINUVIN 292, TINUVIN 770, IRGANOX 1010, IRGANOX 1098 (trade names, respectively sold by Ciba Specialty Chemicals KK), and the like.

[0062] In some embodiments, component A may also include pigments other than the antirust pigments described above. The pigment may be a spherical, fibrous, flaky or other regular or irregularly shaped material having a micrometer or even nanometer size. Examples of pigments include metal oxides such as titanium dioxide, iron oxide, zirconium oxide, aluminum oxide; mixed metal oxides of two or more metals, the metals including manganese, nickel, titanium, chromium, antimony, magnesium, cobalt, iron or aluminum; oxymetallic compounds such as bismuth vanadate, cobalt aluminate, cobalt zincate; pigments with metallic effects such as aluminum flakes, copper and copper-zinc alloys; pearlescent pigments such as lead carbonate and bismuth oxychloride; talc; and any combination thereof. Preferably, the pigment is titanium dioxide and / or iron oxide.

[0063] The total amount of pigments other than the anti-rust pigment described above may be 0 wt % to 40 wt %, such as 1 wt % to 35 wt %, 2 wt % to 30 wt %, 3 wt % to 25 wt %, 4 wt % to 20 wt %, 5 wt % to 15 wt %, based on the total weight of component A. Further preferably, the amount of each pigment used is independently 0 wt % to 40 wt %, 1 wt % to 30 wt %, 2 wt % to 20 wt %, 3 wt % to 15 wt %, 4 wt % to 10 wt %, based on the total weight of component A.

[0064] In some embodiments, the dispersion medium (solvent or carrier fluid) in component A mainly or primarily comprises water. For example, in some embodiments, the dispersion medium in component A comprises at least about 50 wt %, preferably at least about 60 wt %, more preferably at least 70 wt % and up to about 99 wt %, up to about 100 wt % water based on the total weight of the dispersion medium. For example, the dispersion medium comprises about 80 wt %, about 85 wt %, or about 95 wt % water based on the total weight of the dispersion medium.

[0065] The two-component coating composition of the present application can have relatively few volatile components. In some embodiments, based on the total weight of component A, component A contains 0-15% by weight, preferably 0-12% by weight of solvent (especially organic solvent). For example, based on the total weight of component A, component A contains about 2%, 5%, 7%, 10% by weight of solvent (especially organic solvent). Examples of organic solvents include monohydric alcohols or polyhydric alcohols, such as propanol, butanol, hexanol, benzyl alcohol; glycol ethers or esters, such as diethylene glycol dialkyl ethers, dipropylene glycol dialkyl ethers, ethoxypropanol, butyl glycol, each having a C1-C6 alkyl group; glycols, such as ethylene glycol, propylene glycol; and ketones, such as methyl ethyl ketone, acetone, cyclohexanone; N-methylpyrrolidone, N-ethylpyrrolidone; aromatic or aliphatic hydrocarbons, such as toluene, xylene, or linear or branched aliphatic C6-C12 hydrocarbons. In some embodiments, the organic solvent includes dipropylene glycol butyl ether, propylene glycol diacetate, propylene glycol methyl ether acetate, or any combination thereof.

[0066] In some embodiments, based on the total weight of the A component, the A component comprises:

[0067] 40-80% by weight of a hydroxy-functional polyurethane dispersion,

[0068] 2-20% by weight of anti-rust pigments,

[0069] 0.3-2% by weight of silane coupling agent,

[0070] 0.3-20% by weight of auxiliary agents,

[0071] 0-15 wt% solvent.

[0072] In the two-component coating composition described herein, component B comprises a non-hydrophilic isocyanate curing agent. In some embodiments, the non-hydrophilic isocyanate curing agent comprises an aliphatic diisocyanate, an aromatic diisocyanate, a cycloaliphatic diisocyanate, or any combination thereof. Preferably, the non-hydrophilic isocyanate curing agent comprises an aliphatic diisocyanate.

[0073] Preferably, the NCO content of the non-hydrophilic isocyanate curing agent is in the range of 10 wt % to 30 wt %. Preferably, the NCO content is in the range of 15 wt % to 25 wt %. For example, the NCO content may be 18 wt %, 21 wt %, 22 wt %, 23 wt % or 24 wt %. The NCO content is determined according to DIN EN ISO 11 909.

[0074] Preferably, a low viscosity non-hydrophilic isocyanate curing agent is used. For example, the viscosity of the non-hydrophilic isocyanate curing agent at 23° C. is less than 4000 mPa·s. More preferably, the viscosity of the non-hydrophilic isocyanate curing agent at 23° C. is between 600 and less than 3800 mPa·s. For example, the viscosity of the non-hydrophilic isocyanate curing agent at 23° C. may be 730, 1000, 1500, 2000 or 3000 mPa·s. The above viscosity is determined according to DIN EN ISO 3219 / A.3.

[0075] The non-hydrophilic isocyanate curing agent can be in the form of an oligomer or a homopolymer. The oligomer or homopolymer can be an oligomer or a homopolymer comprising 2 to 8 monomer units. For example, the non-hydrophilic isocyanate curing agent can be a trimer.

[0076] Examples of the non-hydrophilic isocyanate curing agent include isocyanate curing agents based on hexamethylene diisocyanate (HDI), dicyclohexylmethane-4,4′-diisocyanate (HMDI), xylylene diisocyanate (XDI), or tetramethyl-meta-xylylene diisocyanate (TMXDI).

[0077] In some preferred embodiments, the aliphatic diisocyanate is an aliphatic diisocyanate based on hexamethylene diisocyanate (HDI), especially preferably an HDI trimer. Preferably, the aliphatic diisocyanate can include one or more of an asymmetric trimer, a symmetric trimer and a homopolymer based on HDI. Commercially available isocyanate curing agents such as DESMODUR N 3300, 3600 and 3900 can be used.

[0078] Each non-hydrophilic isocyanate curing agent can be used alone or in combination. In some embodiments, the non-hydrophilic isocyanate curing agent can also include a combination of two or more curing agents described above. For example, in an exemplary embodiment, DESMODUR N 3300, 3600 and 3900 in a weight ratio of 1:1:1 can be used as the non-hydrophilic isocyanate curing agent.

[0079] The B component may or may not contain a hydrophilic isocyanate curing agent.

[0080] In some embodiments, component B comprises a hydrophilic isocyanate curing agent. The hydrophilic isocyanate curing agent can be prepared by modification in a manner known in the prior art. Examples of hydrophilic isocyanates include, but are not limited to, hydrophilic isocyanates based on isophorone diisocyanate (IPDI) and HDI types.

[0081] In some embodiments, the weight ratio of the non-hydrophilic isocyanate curing agent to the hydrophilic isocyanate curing agent is in the range of 99:1 to 5:95. Preferably, the weight ratio of the non-hydrophilic isocyanate curing agent to the hydrophilic isocyanate curing agent is in the range of 90:10 to 10:90, more preferably 80:20 to 20:80. For example, the weight ratio of the non-hydrophilic isocyanate curing agent to the hydrophilic isocyanate curing agent is 90:10, 70:30, 50:50, 30:70 or 10:90.

[0082] In the two-component polyurethane coating composition described herein, component B comprises a diluent. The diluent may comprise at least one low boiling point solvent. In this article, boiling point has the general meaning understood by those of ordinary skill in the art. "Boiling point" is understood to be the temperature at which a liquid boils under normal pressure (i.e., 1 bar), i.e., the temperature at which the saturated vapor pressure of the liquid is equal to the external pressure. The boiling point value of a compound can be obtained from scientific literature or reference books.

[0083] Preferably, the boiling point of the low boiling point solvent is 160° C. or lower. For example, the low boiling point solvent comprises one or more of propylene glycol monomethyl ether acetate (PMA), dipropylene glycol dimethyl ether (DMM), methyl ethyl ketone (MEK), acetone, methyl isobutyl ketone, cyclohexanone, toluene, xylene, trimethylbenzene, 100# solvent naphtha, 2-methyl propanol acetate (MPA) and n-butyl acetate (BAC). More preferably, the low boiling point solvent is PMA, MEK or a combination of the two.

[0084] In some preferred embodiments, the weight ratio of the diluent to the non-hydrophilic curing agent is between 30:70 and 90:10. More preferably, the weight ratio of the diluent to the non-hydrophilic curing agent is between 40:60 and 85:15. For example, the weight ratio of the diluent to the non-hydrophilic curing agent can be 45:65, 50:50, 55:45, 60:40, 70:30 or 80:20.

[0085] In the two-component coating composition described herein, the relative amounts of component A and component B can be adjusted as needed. In some embodiments, the mass ratio of component A to component B is 1:1 to 10:1, preferably 1:1 to 10:1, more preferably 2:1 to 8:1, such as 3:1, 4:1, 5:1, 6:1, 7:1.

[0086] According to the present application, the two-component coating composition can be prepared as follows: before application, component A and component B are simply mixed in a mixing device in a predetermined ratio. The mixed coating composition can be applied using various methods familiar to those skilled in the art, including spraying (e.g., air-assisted, airless or electrostatic spraying), brushing, roller coating, overflow coating and dipping. In one embodiment of the present application, the mixed coating composition is applied by spraying. The coating composition can be applied to various wet film thicknesses. In an embodiment of the present application, the wet film thickness preferably provides a dry film thickness of about 40 to about 260 μm, and more preferably about 50 to about 150 μm. It can be cured by air drying the applied coating or by accelerating curing using various drying devices familiar to those skilled in the art (e.g., oven).

[0087] Method for preparing two-component coating composition

[0088] The second aspect of the present application provides a method for preparing a two-component coating composition, comprising mixing component A and component B, characterized in that component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, component B comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of component A relative to the initial fineness after 14 days at 40°C is 10% or less, and the fineness is measured using a fineness plate in accordance with GB / T 1724-2019.

[0089] What has been described in the context of the two-component coating composition also applies to the process for producing the two-component coating composition.

[0090] Coated products

[0091] The third aspect of the present application provides a coated product, characterized in that the coated product comprises: a metallic substrate having at least one main surface; and a two-component coating composition described herein or a cured coating thereof coated on the at least one main surface of the metallic substrate.

[0092] The two-component coating composition of the present application can be directly applied on a substrate, or on a coating on a substrate. In some embodiments, the two-component coating composition of the present application can be used in conjunction with a primer. In this case, the product of the present application includes a substrate, a primer layer, and a coating formed by the two-component coating composition of the present application. In other embodiments of the present application, the two-component coating composition of the present application can be applied without a primer and directly applied on the main surface of the substrate. Preferably, the two-component coating composition of the present application has the advantages of a primer and a topcoat two-in-one, can significantly reduce the complexity of construction, reduce equipment and personnel investment, and also has excellent coating properties (including salt spray resistance, acid resistance, adhesion, etc.).

[0093] As the metal substrate for manufacturing the product of the present application, any suitable metal substrate known in the art can be used. As an exemplary illustration, the metal substrate can include one or more of an iron substrate, an aluminum substrate, a copper substrate, carbon steel, stainless steel, an aluminum-zinc alloy, a galvanized steel substrate, a tin-plated steel substrate, and a phosphated plate.

[0094] Advantageously, the cured coating of the coated article described herein has one or more of the following features: no blistering for at least 500 hours in a neutral salt spray test on an aluminum plate, a phosphated plate, or both at 35°C, no blistering for at least 120 hours in a 5% sulfuric acid solution at 20°C, no blistering for at least 120 hours in a 5% sodium hydroxide solution at 20°C, ΔE does not exceed 1.0 after exposure to a xenon lamp for 1000 hours, and the gloss retention rate at 60° is greater than 80%. In particular, the cured coating of the coated article described herein has a very excellent combination of properties, such as two or more features: no blistering for at least 1000 hours in a neutral salt spray test on an aluminum plate, a phosphated plate, or both at 35°C, no blistering for at least 120 hours in a 5% sulfuric acid solution at 20°C, no blistering for at least 120 hours in a 5% sodium hydroxide solution at 20°C, ΔE does not exceed 1.0 after exposure to a xenon lamp for 1000 hours, and the gloss retention rate at 60° is greater than 80%. Preferably, the cured coating of the coated article described herein does not blister for at least 1000 hours in a neutral salt spray test on an aluminum plate, a phosphated plate, or both at 35°C, does not blister for at least 120 hours in a 5% sulfuric acid solution at 20°C, does not blister for at least 120 hours in a 5% sodium hydroxide solution at 20°C, does not blister after being exposed to a xenon lamp for 1000h, and the light retention rate at 60° is greater than 80%. More preferably, the cured coating of the coated article described herein does not blister for at least 1000 hours in a neutral salt spray test on an aluminum plate, a phosphated plate, or both at 35°C, and even more preferably does not blister for at least 1100 hours. For example, the cured coating of the coated article described herein does not blister for at least 1200 hours in a neutral salt spray test on an aluminum plate, a phosphated plate, or both at 35°C. The inventors believe that such an excellent combination of properties described herein could not be achieved before the present application, and is beyond the knowledge and ability of ordinary technicians in the field.

[0095] According to the present application, the coated article can be prepared, for example, by the following steps: (1) providing a polished metal substrate; (2) using a coating process to sequentially coat and form one or more layers of the coating composition described herein on the metal substrate, and obtaining a cured coating after curing.

[0096] The metal products of the present application can be used for the following end applications, including but not limited to: refrigerated containers and non-refrigerated transport containers (such as dry cargo containers) from suppliers or manufacturers including China International Marine Containers (CIMC), Graaff Transportsysteme Gmbh, Maersk Line, and other suppliers or manufacturers known to those skilled in the art; chassis, trailers (including semi-trailers), rail vehicles, truck bodies, ships, bridges, petrochemical storage tank linings, building skeletons, and prefabricated or ready-made metal parts that require temporary indoor or outdoor corrosion protection during manufacturing. Additional uses include metal corners, channels, beams (such as I-beams), pipes, tubes, plates or other components that can be welded into these or other metal parts.

[0097] Example

[0098] The following examples more specifically describe the disclosure of the present application, and these examples are only used for illustrative explanations, because it is obvious to those skilled in the art to make various modifications and variations within the scope of the present disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight. Moreover, all reagents used in the examples are commercially available and can be used directly without further processing.

[0099] Test Method

[0100] Gloss: 60° gloss was evaluated using a Sheen pinhole glossmeter according to ASTM D523.

[0101] Fineness change rate: After the sample is stored at 40°C for 14 days, the initial fineness before storage and the fineness after storage are measured. The fineness change rate relative to the initial fineness after 14 days at 40°C is calculated. The fineness is measured using a fineness plate in accordance with GB / T 1724-2019.

[0102] Pencil Hardness: Pencil hardness is evaluated using ASTM D3363. Data is reported as the pencil hardness of the last successful test before the coating broke. So, for example, if the coating does not break when tested with a 2H pencil, but breaks when tested with a 3H pencil, the coating is reported as having a 2H pencil hardness.

[0103] Impact resistance: The impact resistance of the paint film is measured according to GB / T 1732-2020.

[0104] Adhesion: Measured according to GB / T3324-2017 (cross-cut method). Use a knife to draw 10 groups of cross-cut grids with a spacing of about 2 mm. Use transparent tape to stick on the surface of the cutouts and press them down before tearing them off. The test is graded from 0 to 5 based on the degree of color shedding in the grids. Grade 0 is the best and grade 5 is the worst.

[0105] Moisture and heat resistance: Measure the moisture and heat resistance of the paint film according to GB / T 1740-2007.

[0106] Salt spray resistance: According to GB / T 1771-2007, measure the salt spray resistance of the paint film. The peeling width is required to be less than 2.5mm.

[0107] Chemical resistance: According to GB 9274-1988, at 20±1℃, immerse the sample in 5% sulfuric acid, 5% sodium hydroxide, gasoline or light oil, and observe whether the sample has blistering, cracking, shedding and other adverse conditions. Record the latest time when no adverse conditions are observed.

[0108] Weathering resistance: Artificial aging machine, xenon lamp 1000h, gloss loss and color difference within 1 level, refer to national standard GB / T 1865-2009 "Artificial weathering of paints and varnishes and artificial radiation exposure to filtered xenon arc radiation".

[0109] Determination of element concentration in the clarified liquid after water washing or acid washing: Refer to GB / T 23991-2009 "Determination of soluble harmful elements in coatings", use 0.07 mol / L hydrochloric acid solution and DI water (deionized water) respectively, extract in a constant temperature water bath oscillating tank at 37°C for 1h, filter to obtain clarified liquid, and analyze the elements (such as Zn, Ca) in the clarified liquid by ICP-OES.

[0110] Examples 1-8

[0111] The two-component coating compositions of Examples 1 to 8 and Comparative Example 1 were prepared. Unless otherwise specified, Bayhydrol U XP 2755 from Covestro was used as the aqueous hydroxy polyurethane dispersion, and Bayhydrol A 2770 was used as the aqueous hydroxy polyacrylate dispersion.

[0112] The calcium ion exchange silica used does not release Zn during the acid washing (or water washing) for 1 hour (ICP-OES cannot detect Zn element). After the calcium ion exchange silica used is washed with water for 1 hour, the concentration of Ca element in the obtained clarified liquid is about 565 mg / kg. In addition, the oil absorption of the calcium ion exchange silica itself is about 80 g / 100 g, the average particle size is about 3±0.5 μm, and the pH in the water suspension (10 weight%) is 9.3±0.5.

[0113] According to the components and amounts shown in Table 1 below, component A and component B were prepared respectively, and mixed to obtain a two-component coating composition.

[0114] The obtained coating composition was coated on an aluminum plate and cured. The properties of the coating composition and the coating were tested and the results are shown in Table 2 below.

[0115]

[0116]

[0117] It can be seen from the experimental results that the two-component coating composition of the present application can provide a coating with excellent salt spray resistance, weather resistance, mechanical properties, adhesion and chemical resistance. Moreover, the two-component coating composition of the present application has the characteristics of primer and topcoat two-in-one, simple construction and green environmental protection.

[0118] Although the present application is described with reference to a large number of embodiments and examples, it will be appreciated by those skilled in the art that other embodiments may be designed based on the content disclosed in the present application. It will be readily apparent to those skilled in the art that changes may be made to the present application without departing from the principles disclosed in the foregoing specification. For example, without departing from the principles disclosed in the foregoing specification, a plurality of features or preferred embodiments described herein may be combined, and the resulting technical solutions should be understood to belong to the content recorded herein. Unless otherwise specified in the claims, such changes are deemed to be included in the claims. Accordingly, the embodiments detailed herein are merely exemplary and are not intended to limit the scope of the present application, which is the full scope of the attached claims and any and all equivalents thereof.

Claims

1. A two-component coating composition comprising component A and component B, characterized in that: The A component comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, the B component comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of the A component relative to the initial fineness after 14 days at 40° C. is 10% or less, and the fineness is measured using a fineness plate according to GB / T 1724-2019.

2. The two-component coating composition according to claim 1, characterized in that The hydroxyl-functional polyurethane dispersion has a hydroxyl value of 40-200 mg KOH / g.

3. The two-component coating composition according to claim 1 or 2, characterized in that: The average particle size of the hydroxyl functional polyurethane dispersion is 10-80 nm.

4. The two-component coating composition according to any one of claims 1 to 3, characterized in that Based on the total weight of the A component, the amount of the anti-rust pigment is 2 wt% to 20 wt%, and the amount of the hydroxyl functional polyurethane dispersion is 40 wt% to 80 wt%.

5. The two-component coating composition according to any one of claims 1 to 4, characterized in that The anti-rust pigment comprises calcium ion-exchanged silica, and the calcium content in the anti-rust pigment is 0.5 wt % to 15 wt % on a dry basis.

6. The two-component coating composition according to any one of claims 1 to 5, characterized in that The oil absorption of the anti-rust pigment is 20-100g / 100g.

7. The two-component coating composition according to any one of claims 1 to 6, characterized in that The particle size of the anti-rust pigment is 1.8-20 μm.

8. The two-component coating composition according to any one of claims 1 to 7, characterized in that The pH of the anti-rust pigment is 7-10.

9. The two-component coating composition according to any one of claims 1 to 8, characterized in that The A component comprises one or more of wollastonite, strontium phosphate, zinc phosphate and zinc oxide.

10. The two-component coating composition according to any one of claims 1 to 9, characterized in that The A component includes a silane coupling agent, and preferably, the silane coupling agent is an epoxy silane coupling agent.

11. The two-component coating composition according to any one of claims 1 to 10, characterized in that The weight ratio of the A component to the B component is 1:1 to 10:

1.

12. The two-component coating composition according to any one of claims 1 to 11, characterized in that Based on the total weight of component A, component A comprises: 40-80% by weight of a hydroxy-functional polyurethane dispersion, 2-20% by weight of anti-rust pigments, 0.2-2% by weight of silane coupling agent, 0.3-20% by weight of auxiliary agents, 0-15 wt% solvent.

13. A method for preparing a two-component coating composition according to any one of claims 1 to 12, comprising: Mix component A and component B. Characterized in that the component A comprises at least one hydroxyl-functional polyurethane dispersion and an anti-rust pigment, the component B comprises a non-hydrophilic isocyanate curing agent, and the fineness change rate of the component A relative to the initial fineness after 14 days at 40°C is 10% or less, and the fineness is measured using a fineness plate according to GB / T 1724-2019.

14. A coated product, characterized in that: The coated product comprises: A metallic substrate having at least one major surface; and A two-component coating composition according to any one of claims 1 to 12 or a cured coating thereof coated on at least one major surface of the metallic substrate.

15. The coated product according to claim 14, characterized in that The metal substrate includes one or more of an iron substrate, an aluminum substrate, a copper substrate, carbon steel, stainless steel, an aluminum-zinc alloy, a galvanized steel substrate, a tin-plated steel substrate, and a phosphated plate.

16. The coated product according to claim 14 or 15, characterized in that The cured coating of the coated article does not bubble for at least 1000 hours in a neutral salt spray test at 35°C, does not bubble for at least 120 hours in a 5% sulfuric acid solution at 20°C, does not bubble for at least 120 hours in a 5% sodium hydroxide solution at 20°C, and does not bubble after being exposed to a xenon lamp for 1000 hours. The ΔE does not exceed 1.0 and the gloss retention rate at 60° is greater than 80%.

Citation Information

Patent Citations

  • Room Temperature Crosslinking Coating Composition

    CN107674561A

  • Water-based coating composition

    CN108137986A

  • Two-component polyurethane coating composition, coating formed therefrom, and coated article

    CN114058256A