UV transfer printing adhesive as well as preparation method and application thereof

By using raw materials such as acrylic monomers and silicone modified resins in UV transfer glue, combined with hyperbranched polyester resin and silica powder, the problems of insufficient stain resistance and environmental protection of UV transfer glue are solved, and high efficiency is achieved. Its anti-pollution and environmental protection properties replace highly hazardous PFAS and reduce production costs.

CN118725815APending Publication Date: 2024-10-01HUNAN SOKAN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410944694.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing UV transfer adhesives have deficiencies in stain resistance and environmental protection. The use of perfluorinated and polyfluoroalkyl substances causes environmental pollution, and their wear resistance is weak, requiring special treatment and high-cost nanofillers.

Method used

It adopts a UV transfer glue formula including acrylic monomer, silicone modified resin, hyperbranched polyester acrylic resin, polydimethylsiloxane and nano-silica and other raw materials. It is improved by organic-inorganic hybrid resin and silica micropowder. Wear and stain resistance, and uses a photoinitiator to achieve curing, replacing PFAS to reduce environmental hazards.

Benefits of technology

It provides long-lasting stain resistance and excellent hand feel, improves product protection and quality, and at the same time overcomes the problem of environmental pollution, achieves stain resistance and chemical resistance comparable to PFAS, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004945277740000011
    Figure HDA0004945277740000011
  • Figure HDA0004945277740000012
    Figure HDA0004945277740000012
Patent Text Reader

Abstract

The invention discloses UV transfer printing glue as well as a preparation method and application thereof. The UV transfer printing adhesive is prepared from the following raw materials in parts by weight: 10 to 40 parts of acrylic monomer, 20 to 60 parts of organic silicon modified resin, 5 to 30 parts of organic-inorganic hybrid resin, 5 to 25 parts of hyperbranched polyester acrylic resin, 1 to 15 parts of polydimethylsiloxane, 1 to 20 parts of organic-inorganic hybrid silicon micro powder, 1 to 10 parts of nano silicon dioxide, 1 to 6 parts of additive and 1 to 10 parts of photoinitiator. According to the UV transfer printing adhesive provided by the invention, better wear resistance is obtained by adding and dispersing the organic and inorganic silicon micro powder; meanwhile, the reactive polydimethylsiloxane (PDMS) is added into the formula and is matched with the organic silicon modified resin, so that the transfer printing adhesive is endowed with excellent stain resistance and easy-to-clean performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of transfer adhesives, and in particular relates to a UV transfer adhesive and a preparation method and application thereof. Background Art

[0002] UV transfer adhesive refers to a technology that covers a texture film on a substrate coated with glue, presses it with a roller, and then cures it under UV ultraviolet light curing conditions. After the film is torn off, the fine texture structure of the texture film can be copied to a different substrate. UV transfer adhesive can be applied by dispensing or silk-screen printing, and can be transferred using a texture film. It can be formed on the surface of films such as PC, PET, and silicone, or it can be formed on the surface of a film alone. UV transfer adhesive is mainly formed on epoxy composite panels and alloy substrates through a texture film. It is mainly used for exterior protection and decoration of consumer electronics. It can also be used in automobiles and home appliances, such as 3C electronic back covers, protective shells, and automotive decorative parts. The UV transfer adhesive process is simple to operate, high in efficiency, low in VOC, and energy-saving and environmentally friendly.

[0003] Existing related technical solutions use perfluoro and polyfluoroalkyl substances (PFAS) to achieve excellent stain resistance, relying on fluorine-modified resins or additives. However, PFAS degrades slowly in the natural environment, pollutes groundwater and drinking water, and accumulates in the ecosystem to cause environmental damage. PFAS will accumulate in the human body, damage human health, and has biological toxicity and carcinogenicity. The existing technical solutions generally change the surface tension of the paint film by adjusting the formula, mainly adjusting the proportion of hydrophobic and oleophobic components in the formula, but are limited by the design of the formula, and the use is relatively fixed and single. Related solutions rely on resins for wear resistance or require special treatment, such as resins with nanofillers. The former is weaker in wear resistance than formulas containing wear-resistant fillers, and the latter requires special treatment to pre-disperse the nanofillers in the corresponding resin, which has high cost and process requirements. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a UV transfer adhesive, which can provide long-lasting anti-fouling ability and excellent hand feel, improve product protection ability and quality, and overcome the problem of environmental pollution.

[0005] The invention also provides a method for preparing the UV transfer adhesive.

[0006] The invention also provides a method for preparing a UV-curing paint film.

[0007] The invention also provides a UV curing paint film.

[0008] The invention also provides application of the UV transfer adhesive.

[0009] According to a first aspect of the present invention, a UV transfer adhesive is provided, which comprises the following raw materials in parts by weight: 10 to 40 parts of acrylic monomer, 20 to 60 parts of silicone modified resin, 5 to 30 parts of organic-inorganic hybrid resin, 5 to 25 parts of hyperbranched polyester acrylic resin, 1 to 15 parts of polydimethylsiloxane, 1 to 20 parts of organic-inorganic hybrid silicon powder, 1 to 10 parts of nano-silicon dioxide, 1 to 6 parts of auxiliary agent and 1 to 10 parts of photoinitiator.

[0010] In some embodiments of the present invention, the UV transfer adhesive comprises the following raw materials in parts by weight: 15 to 25 parts of acrylic monomer, 25 to 50 parts of silicone modified resin, 8 to 25 parts of organic-inorganic hybrid resin, 8 to 20 parts of hyperbranched polyester acrylic resin, 1 to 10 parts of polydimethylsiloxane, 3 to 15 parts of organic-inorganic hybrid silicon powder, 3 to 8 parts of nano-silicon dioxide, 1 to 5 parts of additives and 2 to 8 parts of photoinitiator.

[0011] In some preferred embodiments of the present invention, the UV transfer adhesive comprises the following raw materials in parts by weight: 16 to 20 parts of acrylic monomer, 30 to 40 parts of silicone modified resin, 10 to 20 parts of organic-inorganic hybrid resin, 10 to 16 parts of hyperbranched polyester acrylic resin, 2 to 6 parts of polydimethylsiloxane, 5 to 10 parts of organic-inorganic hybrid silicon powder, 5 to 6 parts of nano-silicon dioxide, 1 to 3 parts of additives and 3 to 5 parts of photoinitiator.

[0012] In some embodiments of the present invention, the acrylic monomer includes at least one of 1,6-hexanediol diacrylate (HDDA), acryloyl morpholine (ACMO), trimethylolpropane triacrylate (TMPTA) and pentaerythritol triacrylate (PET3A).

[0013] In some embodiments of the present invention, the organosilicon-modified resin includes an organosilicon-modified resin containing 6 to 8 functional groups.

[0014] In some preferred embodiments of the present invention, the organosilicon-modified resin includes organosilicon-modified polyurethane acrylate; including but not limited to B868 from Guangdong Boxing New Materials.

[0015] In some embodiments of the present invention, the glass transition temperature (Tg) of the organic-inorganic hybrid resin is 40 to 70°C.

[0016] In some preferred embodiments of the present invention, the glass transition temperature (Tg) of the organic-inorganic hybrid resin is 45-65°C.

[0017] In some embodiments of the present invention, the viscosity of the organic-inorganic hybrid resin is 100-25000 cps / 25°C.

[0018] In some embodiments of the present invention, the organic-inorganic hybrid resin has a Shore hardness of 10 to 35D.

[0019] In some preferred embodiments of the present invention, the Shore hardness of the organic-inorganic hybrid resin is 14-29D.

[0020] In some preferred embodiments of the present invention, the organic-inorganic hybrid resin includes at least one of Changxing Material 601A-35, Changxing Material 601C-35 and Changxing Material 601Q-35.

[0021] In some embodiments of the present invention, the number of functional groups of the hyperbranched polyester acrylic resin is 5-25.

[0022] In some preferred embodiments of the present invention, the number of functional groups of the hyperbranched polyester acrylic resin is 8-18.

[0023] In some embodiments of the present invention, the viscosity of the hyperbranched polyester acrylic resin is 1000-4000 cps / 25°C or 4000-6000 cps / 60°C.

[0024] In some preferred embodiments of the present invention, the hyperbranched polyester acrylic resin includes at least one of Changxing Material DR-E522 and Changxing Material DR-E528.

[0025] In some embodiments of the present invention, the photoinitiator includes at least one of initiator 184 and initiator TPO.

[0026] In some preferred embodiments of the present invention, the photoinitiator is a mixture of initiator 184 and initiator TPO in equal weight proportions.

[0027] In some embodiments of the present invention, the auxiliary agent includes at least one of a defoamer, a dispersant and a leveling agent.

[0028] In some preferred embodiments of the present invention, the defoamer includes at least one of a polymer defoamer, a silicone defoamer, an ester defoamer and a mineral oil defoamer.

[0029] In some more preferred embodiments of the present invention, the polymer defoamer is a polyolefin defoamer; the polyolefin defoamer includes but is not limited to BYK-054.

[0030] In some preferred embodiments of the present invention, the dispersant comprises modified polyurethane.

[0031] In some preferred embodiments of the present invention, the leveling agent includes at least one of an organic silicone leveling agent, a polyether-siloxane leveling agent, a non-ionic associative polyurethane leveling agent and an acrylic copolymer leveling agent.

[0032] In some more preferred embodiments of the present invention, the leveling agent is silicone- and polyether-macromolecule-modified acrylic acid, including but not limited to BYK-3568.

[0033] In some embodiments of the present invention, the polydimethylsiloxane comprises UV reactive polydimethylsiloxane.

[0034] In some preferred embodiments of the present invention, the viscosity of the polydimethylsiloxane is 50 to 3000 cps.

[0035] In some preferred embodiments of the present invention, the average molecular weight of the polydimethylsiloxane is 300 to 4000 g / mol.

[0036] In some embodiments of the present invention, the weight ratio of the organosilicon modified resin to the organic-inorganic hybrid resin is (1-5):1.

[0037] In some preferred embodiments of the present invention, the weight ratio of the organosilicon-modified resin to the organic-inorganic hybrid resin is (1.5-4):1.

[0038] In some embodiments of the present invention, the organic-inorganic hybrid silicon micropowder includes at least one of non-reactive organic-inorganic hybrid silicon micropowder and reactive organic-inorganic hybrid silicon micropowder.

[0039] In some preferred embodiments of the present invention, the organic component in the organic-inorganic hybrid silicon micropowder includes polyurethane or acrylic substances.

[0040] In some preferred embodiments of the present invention, the inorganic component in the organic-inorganic hybrid silicon micropowder includes silicon dioxide.

[0041] In some preferred embodiments of the present invention, the average particle size of the organic-inorganic hybrid silicon powder is 2 to 15 μm.

[0042] In some more preferred embodiments of the present invention, the average particle size of the organic-inorganic hybrid silicon powder is 3 to 10 μm.

[0043] In some preferred embodiments of the present invention, the molecular structure of the organic-inorganic hybrid silicon powder includes at least one of a ladder shape, a cage shape and a spherical shape.

[0044] According to a second aspect of the present invention, a method for preparing the UV transfer adhesive as described in the first aspect of the present invention is provided, and the preparation method comprises the following steps:

[0045] The preparation method is prepared by uniformly mixing acrylic monomer, organosilicon modified resin, organic-inorganic hybrid resin, hyperbranched polyester acrylic resin, polydimethylsiloxane, organic-inorganic hybrid silicon micropowder, nano silicon dioxide, auxiliary agent and photoinitiator.

[0046] In some embodiments of the present invention, the preparation method comprises:

[0047] A1: weigh the photoinitiator, acrylic monomer, auxiliary agent and polydimethylsiloxane, and stir and mix them to obtain solution A;

[0048] A2: Weigh the organosilicon modified resin, the organic-inorganic hybrid resin and the hyperbranched polyester acrylic resin, add them to the solution A, and stir to mix well to obtain a solution B;

[0049] A3: Weigh organic-inorganic hybrid silicon micropowder and nano-silicon dioxide, add them into solution B, and stir to mix well to obtain UV transfer adhesive.

[0050] In some preferred embodiments of the present invention, the stirring and mixing temperature in step A1 is 20-30°C.

[0051] In some preferred embodiments of the present invention, the rotation speed of the stirring and mixing in step A1 is 800-1000 rpm.

[0052] In some preferred embodiments of the present invention, the stirring and mixing time in step A1 is 30 to 50 minutes.

[0053] In some preferred embodiments of the present invention, the stirring and mixing temperature in step A2 is 20-30°C.

[0054] In some preferred embodiments of the present invention, the stirring and mixing in step A2 is performed at a speed of 800 to 1000 rpm.

[0055] In some preferred embodiments of the present invention, the stirring and mixing time in step A2 is 15 to 20 minutes.

[0056] In some preferred embodiments of the present invention, the stirring and mixing temperature in step A3 is 40-50°C.

[0057] In some preferred embodiments of the present invention, the rotation speed of the stirring and mixing in step A3 is 1500-2000 rpm.

[0058] In some preferred embodiments of the present invention, the stirring and mixing time in step A3 is 30 to 50 minutes.

[0059] According to a third aspect of the present invention, a method for preparing a UV-curable paint film is provided, the method comprising the following steps:

[0060] S1: The UV transfer adhesive is evenly coated on the substrate, and the surface of the UV transfer adhesive is covered with a texture film to obtain sample A;

[0061] S2: using ultraviolet light to preliminarily cure the sample A obtained in step S1 to obtain a sample B;

[0062] S3: Remove the texture film and use a high-pressure mercury lamp to perform secondary curing on the sample B obtained in step S2 to obtain a UV-cured paint film.

[0063] In some embodiments of the present invention, the substrate in step S1 includes an epoxy composite sheet or an alloy substrate.

[0064] In some preferred embodiments of the present invention, the epoxy composite board comprises an epoxy composite board made of glass fiber or carbon fiber.

[0065] In some preferred embodiments of the present invention, the alloy procurement includes titanium alloy or aluminum alloy.

[0066] In some embodiments of the present invention, the coating method in step S1 includes screen printing. In some preferred embodiments of the present invention, the screen printing has a mesh size of 100 to 200 meshes.

[0067] In some more preferred embodiments of the present invention, the screen printing screen has a mesh count of 150 meshes.

[0068] In some embodiments of the present invention, the coating thickness of the transfer adhesive on the surface of the substrate in step S1 is 20-30 μm.

[0069] In some embodiments of the present invention, the covering texture film in step S1 is performed using a laminating machine.

[0070] In some preferred embodiments of the present invention, the laminating machine comprises a cold laminating machine.

[0071] In some embodiments of the present invention, the step S1 further comprises exhausting air from the contact surface after covering the texture film.

[0072] In some embodiments of the present invention, the ultraviolet light in step S2 is near ultraviolet light.

[0073] In some preferred embodiments of the present invention, the near-ultraviolet light is 395 nm ultraviolet light.

[0074] In some embodiments of the present invention, the energy of the ultraviolet light in step S2 is 1000-2000 mJ / cm 2 .

[0075] In some embodiments of the present invention, the intensity of the ultraviolet light in step S2 is 1000-2000 mW / cm 2 .

[0076] In some preferred embodiments of the present invention, the intensity of the ultraviolet light in step S2 is 1500 mW / cm 2 .

[0077] In some embodiments of the present invention, the energy of the high pressure mercury lamp for curing in step S3 is 800-1000 mJ / cm 2 .

[0078] In some embodiments of the present invention, the light intensity of the high pressure mercury lamp used for curing in step S3 is 90 to 120 mW / cm 2 .

[0079] In some preferred embodiments of the present invention, the light intensity of the high pressure mercury lamp used for curing in step S3 is 108 mW / cm 2 .

[0080] In some embodiments of the present invention, the UV-cured paint film is prepared by using the UV transfer adhesive described in the first aspect of the present invention.

[0081] In some embodiments of the present invention, the textured film includes a silicone film or a glass film coated with a stain-resistant layer.

[0082] In some preferred embodiments of the present invention, the anti-fouling layer includes an organic silicon coating or a fluorine-containing coating.

[0083] According to a fourth aspect of the present invention, a UV-curing paint film is provided. The UV-curing paint film is prepared by the preparation method described in the third aspect of the present invention.

[0084] In some embodiments of the present invention, the water drop angle of the UV-cured paint film is 80° to 130°.

[0085] According to a fifth aspect of the present invention, a use of the UV transfer adhesive as described in the first aspect of the present invention in preparing a stain-resistant and wear-resistant paint film is proposed.

[0086] In some embodiments of the present invention, the water drop angle of the stain-resistant and wear-resistant paint film is 80° to 130°.

[0087] The present invention has at least the following beneficial effects:

[0088] 1) The UV transfer adhesive provided by the present invention obtains better wear resistance by adding and dispersing organic and inorganic silicon powder; at the same time, reactive polydimethylsiloxane (PDMS) is added to the formula, and the organic silicon modified resin is matched to give the transfer adhesive excellent stain resistance and easy cleaning performance; the addition of hyperbranched polyester resin ensures that the transfer adhesive has a high cross-linking degree while making the transfer adhesive have strong toughness, and the hard but brittle characteristics of the UV transfer adhesive are improved;

[0089] 2) The UV transfer adhesive provided by the present invention uses PDMS instead of PFAS, that is, silicon (Si) is used to replace fluorine (F), so that the product has the same performance as PFAS in terms of stain resistance and chemical resistance, and PDMS overcomes the defect of PFAS in terms of environmental damage;

[0090] 3) The UV transfer adhesive provided by the present invention uses commercial micron-grade fillers, which can be dispersed and prepared by a high-speed disperser without additional processing; the organic and inorganic silicon powder is well dispersed in the system, and combined with the organic silicone resin and the organic and inorganic hybrid resin, the wear resistance of the paint film is enhanced;

[0091] 4) The UV-cured paint film provided by the present invention can provide long-lasting anti-fouling ability, wear resistance and excellent hand feel, thereby improving the product protection ability and quality;

[0092] 5) The preparation method of the UV-curable paint film provided by the present invention can induce different components in the paint film to form a gradient distribution through the texture film, thereby realizing the regulation of its surface tension. When using the same formula, different paint film surface tensions can still be achieved through the texture film, which greatly improves the flexibility and scope of formula use. BRIEF DESCRIPTION OF THE DRAWINGS

[0093] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0094] Figure 1 This is a graph showing the test results of the water drop angle of paint films with different formulations in the test examples of the present invention;

[0095] Figure 2 This is a graph showing the test results of the wear resistance of paint films with different formulations in the test examples of the present invention. DETAILED DESCRIPTION

[0096] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0097] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0098] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0099] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0100] Example 1

[0101] The present embodiment provides a UV transfer adhesive, and the preparation method of the UV transfer adhesive specifically comprises the following steps (the following raw material amounts are all expressed in parts by weight):

[0102] 1) Weigh 5 parts of photoinitiator and add them into a container, add 16 parts of acrylic monomer, 1 part of auxiliary agent and 2 parts of reactive polydimethylsiloxane (PDMS) thereto, stir at 900 rpm (800-1000 rpm) for 40 min (30-50 min) at room temperature (25°C) to obtain a homogeneous solution A; wherein the photoinitiator is a mixture of initiator 184 and initiator TPO in equal weight proportions; the auxiliary agent is a defoamer (polyolefin defoamer purchased from BYK Chemical The mixture is a mixture of a defoamer (defoaming agent, purchased from Shanghai Tiger Polymer Technology Co., Ltd., model BYK-054), a dispersant (modified polyurethane dispersant, purchased from BASF, model EFKA-4010) and a leveling agent (organic acrylic acid modified with silicone and polyether, purchased from BYK, model BYK-3568), the mixing mass ratio of defoamer: dispersant: leveling agent = 1:2:1; PDMS was purchased from Shanghai Tiger Polymer Technology Co., Ltd., model number tech-2240, with a viscosity of 50-3000cps and an average molecular weight of 300-4000g / mol.

[0103] 2) Add 40 parts of organosilicon modified resin (purchased from Boxing New Materials, model B868), 10 parts of organic-inorganic hybrid resin (purchased from Changxing Materials, model 601A-35) and 16 parts of hyperbranched polyester acrylic resin (purchased from Changxing Materials, model DR-E522) to the solution A obtained in step 1), and stir at 900 rpm (800-1000 rpm) for 18 min (15-20 min) at room temperature (25°C) to obtain a homogeneous solution B; wherein the organosilicon modified resin is a resin with 6 functional groups.

[0104] 3) Add 5 parts of organic-inorganic hybrid silicon micropowder and 5 parts of nano-silicon dioxide to the solution B obtained in step 2), stir at 45°C (40-50°C) and 1800 rpm (1500-2000 rpm) for 40 min (30-50 min), and stir evenly to obtain a UV transfer adhesive; wherein the organic-inorganic hybrid silicon micropowder is a non-reactive organic-inorganic hybrid silicon micropowder (purchased from Momentive, model TOSPEARL 2000B), and its molecular structure is spherical.

[0105] Example 2

[0106] This embodiment provides a UV transfer adhesive. The preparation method of the UV transfer adhesive is different from that of Embodiment 1 only in that the ratio of raw materials is adjusted, and other steps are the same. The weight ratio of raw materials used in this embodiment is as follows:

[0107] 20 parts of acrylic monomer, 30 parts of organosilicon modified resin, 10 parts of organic-inorganic hybrid resin, 16 parts of hyperbranched polyester acrylic resin, 6 parts of polydimethylsiloxane, 5 parts of organic-inorganic hybrid silicon powder, 5 parts of nano-silicon dioxide, 3 parts of auxiliary agent and 5 parts of photoinitiator.

[0108] Example 3

[0109] This embodiment provides a UV transfer adhesive. The preparation method of the UV transfer adhesive is different from that of Embodiment 1 only in that the ratio of raw materials is adjusted, and other steps are the same. The weight ratio of raw materials used in this embodiment is as follows:

[0110] 17 parts of acrylic monomer, 30 parts of organosilicon modified resin, 20 parts of organic-inorganic hybrid resin, 10 parts of hyperbranched polyester acrylic resin, 2 parts of polydimethylsiloxane, 10 parts of organic-inorganic hybrid silicon powder, 6 parts of nano-silica, 2 parts of auxiliary agent and 3 parts of photoinitiator.

[0111] Example 4

[0112] This embodiment provides a UV-curable paint film, which is prepared by combining a highly stain-resistant, wear-resistant, fluorine-free UV-curable transfer adhesive provided in Example 1 with a textured film made of silicone material. The preparation method of the UV-curable paint film specifically includes the following steps:

[0113] 1) The UV transfer adhesive provided in Example 1 is uniformly coated on the titanium alloy substrate by screen printing, and the mesh number is 150 meshes; the coating thickness of the transfer adhesive on the surface of the substrate is 25 μm (20-30 μm is acceptable);

[0114] 2) Covering the surface of the transfer adhesive with a texture film by a cold laminating machine, and exhausting the air on the contact surface to obtain sample A;

[0115] 3) Using a 395nm wavelength LED lamp, preliminarily cure the sample A obtained in step 2) to obtain sample B. The energy during curing is 1500mJ / cm 2 (1000~2000mJ / cm 2 The light intensity is 1500mW / cm 2 ;

[0116] 4) Remove the texture film and use a high-pressure mercury lamp to perform secondary curing on the sample B that was initially cured in step 3). The energy during curing is 900mJ / cm 2 (800~1000mJ / cm 2 The light intensity is 108mW / cm 2 , and obtain the final cured UV-cured paint film.

[0117] Example 5

[0118] This embodiment provides a UV-curable paint film, which is prepared by combining a highly stain-resistant, wear-resistant, fluorine-free UV-curable transfer adhesive provided in Example 1 with a glass film coated with a silicone stain-resistant layer. The specific steps are consistent with those in Example 4.

[0119] Comparative Example 1

[0120] This comparative example provides a UV-cured paint film, which is prepared by combining a highly stain-resistant, wear-resistant, fluorine-free UV-cured transfer adhesive provided in Example 1 with a textured film made of polyethylene terephthalate (PET), and the specific steps are consistent with those of Example 4.

[0121] Comparative Example 2

[0122] This comparative example provides a UV-cured paint film, which is prepared by combining a highly stain-resistant, wear-resistant, fluorine-free UV-cured transfer adhesive provided in Example 1 with a textured film made of polycarbonate (PC), and the specific steps are consistent with those in Example 4.

[0123] Test example

[0124] This test example tests the performance of the highly stain-resistant, wear-resistant, fluorine-free UV-curable transfer adhesive provided by the present invention and the UV-curable paint film prepared based on the transfer adhesive. The specific test method and test results are as follows:

[0125] 1. Test the effect of PDMS and PFAS on the water drop angle of paint film:

[0126] This test example is based on the raw material ratio of the UV transfer adhesive provided in Example 2, and uses 4 different types of PDMS and 1 PFAS of equal quality to replace the PDMS in Example 2 to obtain 4 groups of UV transfer adhesives (PDMS1 group to PDMS4 group), and selects a glass texture film coated with a silicone anti-fouling layer. Referring to the paint film preparation method provided in Example 4, PDMS1 to PDMS4 and the UV transfer adhesive obtained in Example 2 are used to prepare UV transfer paint films;

[0127] This test example tested the water drop angles of the above five groups of paint films and the control group of paint films (PDMS was omitted based on the UV transfer adhesive ratio of Example 2), and compared the effects of PDMS and PFAS on the water drop angles of the paint films. The test steps were based on the national standard GB / T 30693-2014.

[0128] Among them, the PFAS used is a UV acrylic monomer modified with organic fluorine (purchased from Zhongshan Jieshida); PDMS1~PDMS4 groups all use 1-2 functional group reactive PDMS purchased from Tiger Additives, and the models are Tech-2205 (single functional group, molecular weight 300~400g / mol), Tech-2220 (double functional group, molecular weight 1000~2000g / mol), Tech-2340 (double functional group, molecular weight about 4000g / mol) and Tech-2240 (double functional group, molecular weight about 4000g / mol). The test results are as follows: Figure 1 shown.

[0129] Depend on Figure 1 It can be seen that the water drop angles of the preferred PDMS4 group and PFAS group are basically the same, namely 121° and 125°, respectively, on the basis of the same distribution ratio and preparation process of other components. This shows that the highly stain-resistant, wear-resistant and fluorine-free UV-curable transfer adhesive provided by the present invention overcomes the problem of environmental pollution by replacing PFAS with PDMS, and maintains excellent stain resistance.

[0130] 2. Test the effect of texture films of different materials on the surface tension of the paint film:

[0131] Based on the UV transfer glue provided in Example 1 and under the process parameters provided in Example 4, a high-gloss textured film made of different materials without texture (the surface of the textured film is flat and textureless, which can avoid the influence of the texture structure on the test results) can be used to induce the gradient distribution of different components in the formula through surface tension, thereby adjusting the surface tension of the paint film.

[0132] Surface tension can also be detected by measuring the angle of water droplets. The smaller the angle of the water droplets, the greater the surface tension.

[0133] The specific test steps refer to the international standard D-2578 formulated by the American Society for Testing and Materials (ASTM). The water drop angle test results of Comparative Examples 1-2 and Example 4 are shown in Table 1.

[0134] Table 1 Surface tension of paint films made of textured films of different materials

[0135] Group Comparative Example 1 (PET) Comparative Example 2 (PC) Example 4 (Silica gel) Water drop angle 84° 97° 105°

[0136] As shown in Table 1, the water drop angle of the paint film can be adjusted from 84° to 97°, and then to 105°. The value of the water drop angle can be controlled by the material of the texture film without changing the formula; the surface tension of PET material is known to be 35.6mJ / m 2 The surface tension of PC material is 29.3mJ / m 2 The surface tension of silicone material is 20.5mJ / m 2 It can be seen that the greater the surface tension of the texture film itself, the greater the surface tension of the corresponding paint film prepared.

[0137] 3. Test the effect of different fillers on the wear resistance of paint film:

[0138] The wear resistance is mainly analyzed by rubber wear test. This test example uses CS-17 rubber to test the change of glossiness of the paint film after rubber friction with different fillers. Specifically, the filler-free group, organic-inorganic hybrid silicon powder group 1, organic-inorganic hybrid silicon powder group 2 and ceramic powder group were tested.

[0139] The filler-free group was obtained by omitting the organic-inorganic hybrid silicon powder based on the formula of Example 3, and the other raw material components were consistent with those of Example 3;

[0140] Organic-inorganic hybrid silicon micropowder group 1 uses organic-inorganic hybrid silicon micropowder (purchased from Dow Corning, model Dow Corning 23, average particle size 5 μm) whose main component is epoxy-modified silicone elastomer powder. Except for the replacement of the type of organic-inorganic hybrid silicon micropowder, the other raw material ratios are the same as those in Example 3;

[0141] Organic-inorganic hybrid silicon micropowder group 2 uses organic-inorganic hybrid silicon micropowder whose main component is spherical silicone resin powder (i.e., the UV transfer adhesive formula provided in Example 3);

[0142] The ceramic powder group is obtained by replacing the organic-inorganic hybrid silicon powder in Example 3 with ceramic powder of equal mass, and the other raw material components are the same as those in Example 3.

[0143] The steps of the rubber wear test include: testing the gloss of each group of samples after 0, 25, 50, 100 and 200 cycles, with a test load of 1kg and 25 cycles per minute. For specific test steps, please refer to the international standard D1044-99 formulated by the American Society for Testing and Materials (ASTM); the smaller the gloss change, the better the wear resistance; the results are as follows: Figure 2 shown.

[0144] Depend on Figure 2 It can be seen that compared with the filler-free group, the organic-inorganic hybrid silicon micropowder group 1 and group 2 have a significant improvement in wear resistance. The glossiness change of the ceramic powder is higher than that of the filler-free group, and the wear resistance effect is worse, indicating that the present invention greatly improves the wear resistance of the paint film by adding organic-inorganic hybrid silicon micropowder.

[0145] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A UV transfer adhesive, It is characterized in that The UV transfer adhesive comprises the following raw materials in parts by weight: 10-40 parts of acrylic monomer, 20-60 parts of organosilicon modified resin, 5-30 parts of organic-inorganic hybrid resin, 5-25 parts of hyperbranched polyester acrylic resin, 1-15 parts of polydimethylsiloxane, 1-20 parts of organic-inorganic hybrid silicon powder, 1-10 parts of nano silicon dioxide, 1-6 parts of auxiliary agent and 1-10 parts of photoinitiator.

2. The UV transfer adhesive according to claim 1, It is characterized in that The acrylic monomer includes at least one of 1,6-hexanediol diacrylate, acryloyl morpholine, trimethylolpropane triacrylate and pentaerythritol triacrylate; And / or, the glass transition temperature of the organic-inorganic hybrid resin is 40-70°C.

3. The UV transfer adhesive according to claim 1, It is characterized in that The number of functional groups of the hyperbranched polyester acrylic resin is 5 to 25; And / or, the photoinitiator includes at least one of the initiator 184 and the initiator TPO.

4. The UV transfer adhesive according to claim 1, It is characterized in that The polydimethylsiloxane includes UV reactive polydimethylsiloxane; And / or, the auxiliary agent includes at least one of a defoamer, a dispersant and a leveling agent.

5. The UV transfer adhesive according to claim 1, It is characterized in that The organic-inorganic hybrid silicon micropowder includes at least one of non-reactive organic-inorganic hybrid silicon micropowder and reactive organic-inorganic hybrid silicon micropowder; Preferably, the organic component of the organic-inorganic hybrid silicon powder includes polyurethane or acrylic substances; Preferably, the inorganic component in the organic-inorganic hybrid silicon micropowder includes silicon dioxide; Preferably, the average particle size of the organic-inorganic hybrid silicon powder is 2 to 15 μm.

6. A method for preparing a UV transfer adhesive as claimed in any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: The preparation method is prepared by uniformly mixing acrylic monomer, organosilicon modified resin, organic-inorganic hybrid resin, hyperbranched polyester acrylic resin, polydimethylsiloxane, organic-inorganic hybrid silicon micropowder, nano silicon dioxide, auxiliary agent and photoinitiator.

7. A method for preparing a UV-curable paint film, It is characterized in that The preparation method comprises the following steps: S1: The UV transfer adhesive is evenly coated on the substrate, and the surface of the UV transfer adhesive is covered with a texture film to obtain sample A; S2: using ultraviolet light to preliminarily cure the sample A obtained in step S1 to obtain a sample B; S3: Remove the texture film and use a high-pressure mercury lamp to perform secondary curing on the sample B obtained in step S2 to obtain a UV-cured paint film.

8. The preparation method according to claim 7, It is characterized in that The textured film includes a silicone film or a glass film coated with a stain-resistant layer; Preferably, the anti-fouling layer comprises a silicone coating or a fluorine-containing coating.

9. A UV curing paint film, It is characterized in that The UV-cured paint film is prepared by the preparation method described in claim 7.

10. Use of the UV transfer adhesive as claimed in any one of claims 1 to 5 in preparing stain-resistant and wear-resistant paint films.