Thermochromic luminescent material as well as preparation method and application thereof
By doping RbCdCl3 with manganese ions, the reversible thermochromic properties of lead-free thermochromic luminescent materials are achieved, which solves the toxicity and instability problems of lead-based halides and is suitable for the fields of intelligent response and temperature detection.
Patent Information
- Application Number
- CN202410793935.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Existing thermochromic luminescent materials suffer from lead toxicity and instability issues, and traditional lead halide perovskites are not environmentally friendly in commercial applications, resulting in an urgent need to explore new lead-free thermochromic luminescent materials.
By doping a very small amount of manganese ions in the RbCdCl3 crystal structure, inducing exciton self-trapping and spin-forbidden d-d transition of Mn2+ ions, differential luminescence at room temperature and 420K is achieved, demonstrating reversible thermochromic luminescence characteristics, and using water The material is synthesized by a thermal reaction method, which solves the problems of toxicity and instability of lead-based halides.
It has achieved reversible thermochromic luminescence characteristics at room temperature and high temperature. The material shows obvious alternating emission of red and yellow light when the temperature changes. It has excellent fluorescence intensity and quantum yield and is suitable for intelligent response luminescence, anti-counterfeiting and Temperature detection field.
Smart Images

Figure CN118725856A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermochromic luminescent materials, and more specifically to a thermochromic luminescent material and a preparation method and application thereof. Background Art
[0002] Spectrally responsive thermochromic luminescent materials (TLMs) have attracted extensive attention due to their cutting-edge applications in temperature visualization and sensing technologies. Thermocouples and infrared thermometers are commonly used on the market, both of which have their limitations. In devices using electromagnetic induction heating, traditional thermocouples are not suitable for use due to material limitations, while limited penetration and inevitable background signal interference will also limit the scope of use of infrared thermometers. Luminescent metal halide perovskites have attracted great research interest in the field of optoelectronics due to their color tunability and inexpensive synthesis process. The emission color of TLMs will show reversible changes with temperature, and the application of luminescent materials and thermochromic materials can be combined for optical temperature indicators.
[0003] There have been many studies and reports on metal halides (CsPbX3) in the field of thermochromism. However, due to the toxicity of traditional lead halide perovskites, they are not environmentally friendly in actual commercial applications and can cause serious health problems even under extremely low exposure conditions. In recent years, researchers have been committed to the development of lead-free halide thermochromic luminescent materials, but the types of publicly reported thermochromic luminescent materials are still relatively small. Therefore, the exploration of new lead-free, stable and easily controllable metal halide materials has received a lot of attention. Summary of the invention
[0004] In order to solve the above problems, the first object of the present invention is to provide a thermochromic luminescent material. The thermochromic luminescent material provided by the present invention partially replaces the cadmium ions in the RbCdCl3 crystal structure with a very small amount of manganese ions, thereby inducing exciton self-trapping and Mn 2+ The spin of the ions prohibits dd transitions, thereby achieving differentiated luminescence at room temperature and 420K, showing obvious reversible thermochromic luminescence properties.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned thermochromic luminescent material. The present invention has a simple synthesis process, mild reaction conditions, abundant raw material sources, low prices, solves the lead toxicity and instability problems in lead-based halide crystals, and is expected to be widely used in the fields of intelligent response luminescence, anti-counterfeiting and temperature measurement.
[0006] The third object of the present invention is to provide an application of the above-mentioned thermochromic luminescent material in intelligent response luminescence, anti-counterfeiting and temperature detection.
[0007] A fourth object of the present invention is to provide an anti-counterfeiting material.
[0008] A fifth object of the present invention is to provide a temperature detection device.
[0009] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0010] The present invention discloses a thermochromic luminescent material, the chemical formula of which is RbCd (1-x) Mn x Cl3, colorless needle-shaped single crystal;
[0011] Wherein, x is the mole fraction, and its value range is 0<x≤15%.
[0012] The thermochromic luminescent material provided by the present invention is doped with a very small amount of manganese ions, thereby realizing a response stimulus to the external environment temperature, causing a change in the crystal structure and presenting an obvious reversible thermochromic luminescent property. Specifically, the thermochromic luminescent material belongs to the orthorhombic system at room temperature, the space group is Pnma, the emission peak is located at 575nm, and it exhibits red light emission; when the thermochromic luminescent material is heated to above 420K, its crystal structure becomes a tetragonal system, the space group becomes P4 / mbm, the emission peak is located at 575nm, and it exhibits yellow light emission. Moreover, after the thermochromic luminescent material is restored from a temperature above 420K to room temperature, it is found that the thermochromic luminescent material can still maintain yellow light emission for a long time, that is, it can maintain yellow light emission when placed in the air for 12h, and then gradually changes to red light emission. In a sealed storage (non-vacuum environment), it can maintain yellow light emission for at least 2 days, and then gradually changes to red light emission.
[0013] The thermochromic luminescent material provided by the present invention is excited by ultraviolet light with a wavelength of 200-400nm. The red fluorescence intensity increases with the increase of manganese doping, and the yellow fluorescence intensity increases with the increase of manganese doping. When the chemical formula of the thermochromic luminescent material is RbCd 93.91% Mn 6.09% Cl3, the yellow fluorescence intensity reaches the highest and the quantum yield reaches 100%, confirming that the more symmetrical tetragonal phase is more favorable for Mn 2+ It was also found that the fluorescence intensity of the thermochromic luminescent material increased with the increase of temperature at 160K-420K, showing an obvious anti-thermal quenching effect. Therefore, with its excellent reversible fluorescence color change characteristics, it is expected to be widely used in the fields of intelligent response luminescence, anti-counterfeiting, temperature detection, etc.
[0014] The experiment also found that within the entire range of x, that is, 0<x≤15%, RbCd (1-x) Mnx Cl3 can maintain the original RbCdCl3 crystal structure and show obvious reversible thermochromic performance. From the perspective of thermochromic performance, when the x value range is 0<x≤0.4% and 5≤x≤7%, it can show obvious differentiated luminescence with temperature changes, that is, when the x value range is 0<x≤0.4%, it shows relatively weak red light emission at room temperature and relatively strong yellow light emission at 420K. When the x value range is 5≤x≤7%, it shows strong red light emission at room temperature and relatively stronger yellow light emission at 420K. In the above range, obvious luminescence color change can be observed. In a specific embodiment, in order to obtain higher fluorescence intensity and quantum yield, it is advisable to control the x value range to 5-7%.
[0015] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0016] The present invention discloses a method for preparing the thermochromic luminescent material as described above, comprising the following steps:
[0017] The rubidium-containing compound, the cadmium-containing compound and the manganese-containing compound are mixed, and then placed in a hydrogen chloride solution and heated until dissolved, and then the reaction solution is transferred to a hydrothermal reactor containing a polytetrafluoroethylene liner for hydrothermal reaction. After the reaction is completed, it is cooled, filtered and washed to obtain RbCd (1-x) Mn x Cl3 single crystal.
[0018] Furthermore, the rubidium-containing compound is selected from one or more of rubidium-containing oxides (e.g., rubidium oxide), rubidium-containing hydroxides (e.g., rubidium hydroxide), and rubidium-containing chlorides (e.g., rubidium chloride);
[0019] The cadmium-containing compound is selected from one or more of cadmium-containing oxides (such as cadmium oxide), cadmium-containing hydroxides (such as cadmium hydroxide), and cadmium-containing chlorides (such as cadmium chloride);
[0020] The manganese-containing compound is selected from one or more of a manganese-containing oxide (such as manganese oxide), a manganese-containing hydroxide (such as manganese hydroxide), and a manganese-containing chloride (such as manganese chloride).
[0021] Furthermore, the temperature of the hydrothermal reaction is 360-400K, and the time of the hydrothermal reaction is 2-8h.
[0022] Furthermore, the molar ratio of the rubidium-containing compound, the cadmium-containing compound and the manganese-containing compound is 1:(0.4-0.95):(0.05-0.6). The molar ratio of the manganese-containing compound to the cadmium-containing compound should not be too large, which may affect the crystal form of the final compound, making it difficult to maintain the original RbCdCl3 crystal structure and transform into other crystal phase structures.
[0023] Furthermore, the mass concentration of the hydrogen chloride solution is 20-38%.
[0024] Furthermore, after washing, drying is also included, the drying temperature is 30-50° C., and the drying time is 2-24 hours.
[0025] In order to achieve the third object, the present invention adopts the following technical solutions:
[0026] The present invention discloses an application of the thermochromic luminescent material as described above in intelligent response luminescence, anti-counterfeiting and temperature detection.
[0027] In order to achieve the fourth objective, the present invention adopts the following technical solutions:
[0028] The invention discloses an anti-counterfeiting material comprising the thermochromic luminescent material as described above.
[0029] In order to achieve the fifth object, the present invention adopts the following technical solutions:
[0030] The present invention discloses a temperature detection device comprising the thermochromic luminescent material as described above.
[0031] The beneficial effects of the present invention are as follows:
[0032] The present invention discloses a thermochromic luminescent material, the chemical formula of which is RbCd (1-x) Mn x Cl3, through the doping of a very small amount of manganese ions, the response stimulation to the external environment temperature is achieved, the crystal structure changes and an obvious reversible thermochromic luminescence characteristic is presented. Specifically: the thermochromic luminescent material belongs to the orthorhombic system at room temperature, the space group is Pnma, the emission peak is located at 575nm, and it is red light emission; when the thermochromic luminescent material is heated to above 420K, its crystal structure becomes a tetragonal system, the space group becomes P4 / mbm, the emission peak is located at 575nm, and it is yellow light emission. Moreover, after the thermochromic luminescent material is restored from a temperature above 420K to room temperature, it is found that the thermochromic luminescent material can still maintain yellow light emission for a long time, that is, it can maintain yellow light emission when placed in the air for 12h, and then gradually changes to red light emission. In sealed storage (non-vacuum environment), it can maintain yellow light emission for at least 2 days, and then gradually changes to red light emission.
[0033] The thermochromic luminescent material disclosed in the present invention is excited by ultraviolet light with a wavelength of 200-400nm. The red fluorescence intensity increases with the increase of manganese doping, and the yellow fluorescence intensity increases with the increase of manganese doping. When the chemical formula of the thermochromic luminescent material is RbCd 93.91%Mn 6.09% Cl3, the yellow fluorescence intensity reaches the highest and the quantum yield can reach 100%, which confirms that the more symmetrical tetragonal phase is more conducive to the Mn 2+ of photoluminescence.
[0034] The thermochromic luminescent material disclosed in the present invention has a fluorescence intensity that increases with the increase of temperature during the temperature change from 160K to 420K, showing an obvious anti-thermal quenching effect.
[0035] The thermochromic luminescent material disclosed in the present invention can not only maintain the original crystal structure of RbCdCl3, but also induce exciton self-trapping and Mn 2+ The spin of the ion prohibits dd transition, thereby achieving structural changes in response to external environmental temperature stimulation.
[0036] The present invention also provides a synthesis process, which is simple, has mild reaction conditions, abundant raw material sources, and low prices. It solves the problems of lead toxicity and instability in lead-based halide crystals and is expected to be widely used in the fields of intelligent response luminescence, anti-counterfeiting, and temperature measurement. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0038] Figure 1 It is the X-ray diffraction test spectrum of the samples of Example 1 and Example 5 of the present invention, wherein, Figure 1 a is RbCdCl3- at room temperature and RbCd 93.91% Mn 6.09% The test spectrum of Cl3- at room temperature, Figure 1 b is RbCdCl3-420 K, RbCd 93.91% Mn 6.09% Test spectrum of Cl3-420 K.
[0039] Figure 2 The fluorescence spectra of the samples of Examples 2 to 5 of the present invention are shown in FIG. Figure 2 a in the equation is RbCd 99.65% Mn 0.35% Cl3-room temperature, RbCd 99.50% Mn 0.50% Cl3-room temperature, RbCd 98.84% Mn 1.16% Cl3- Room temperature and RbCd 93.91% Mn 6.09% Fluorescence spectrum of Cl3- at room temperature, Figure 2 b in the figure is RbCd 99.65% Mn 0.35% Cl3-420K、RbCd 99.50% Mn0.50% Cl3-420K、RbCd 98.84% Mn 1.16% Cl3-420K and RbCd 93.91% Mn 6.09% Fluorescence spectrum of Cl3-420K.
[0040] Figure 3 This is the CIE chromaticity coordinate diagram of the sample of Example 5 of the present invention.
[0041] Figure 4 This is a fluorescence temperature-dependent emission spectrum diagram of the sample of Example 5 of the present invention, wherein: Figure 4 a in the equation is RbCd 93.91% Mn 6.09% The fluorescence emission spectrum of Cl3- at room temperature. Figure 4 b in the figure is RbCd 93.91% Mn 6.09% Fluorescence temperature-dependent emission spectrum of Cl3-420K.
[0042] Figure 5 This is a diagram showing the reversible transformation effect between red light emission and yellow light emission achieved by the sample of Example 5 of the present invention under ultraviolet irradiation. DETAILED DESCRIPTION
[0043] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0044] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0045] Example 1
[0046] 0.3628g of rubidium chloride and 2.7498g of cadmium chloride were placed in 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for a hydrothermal reaction and kept warm for 2h. Subsequently, the mixture was naturally cooled to room temperature, filtered, washed, and dried in an oven at 30°C for 6h to obtain colorless needle-shaped crystals of RbCdCl3.
[0047] The crystal structure of the sample of Test Example 1 when it is not heated, that is, the sample at room temperature, is denoted as RbCdCl3-room temperature, and the powder X-ray diffraction pattern is shown in Figure 1 In figure a, single crystal diffraction test shows that RbCdCl3- belongs to the orthorhombic system at room temperature, and its space group is Pnma.
[0048] When the sample of Example 1 was heated to 420K to test its crystal structure, the sample was recorded as RbCdCl3-420K. After single crystal diffraction test, the powder X-ray diffraction pattern was shown. Figure 1 In figure b, RbCdCl3-420K is a tetragonal crystal with a space group of P4 / mbm, indicating that RbCdCl3 exhibits different crystal structures at room temperature and 420K.
[0049] After irradiation and observation with ultraviolet light, RbCdCl3- at room temperature and RbCdCl3- at 420K have no fluorescence properties.
[0050] Example 2
[0051] 0.3628g of rubidium chloride, 2.4748g of cadmium chloride and 0.2969g of manganese chloride tetrahydrate were put into 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for hydrothermal reaction and kept warm for 2h. Subsequently, the temperature was naturally lowered to room temperature, filtered, washed, and dried in an oven at 30℃ for 6h to obtain colorless needle-shaped crystals. The chemical formula of the crystals was RbCd tested by XRD and ICP. 99.65% Mn 0.35% Cl3.
[0052] The crystal structures of the samples of Example 2 were tested respectively before heating (room temperature) and after heating (420K), and the samples were respectively denoted as RbCd 99.65% Mn 0.35% Cl3- Room temperature and RbCd 99.65% Mn 0.35% Cl3-420K, it was found that the crystal structure was consistent with that of Example 1 under the same conditions, indicating that manganese doping did not affect its crystal structure.
[0053] Example 3
[0054] 0.3628g of rubidium chloride, 2.1998g of cadmium chloride and 0.5937g of manganese chloride tetrahydrate were put into 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for hydrothermal reaction and kept warm for 2h. Subsequently, the temperature was naturally lowered to room temperature, filtered, washed, and dried in an oven at 30℃ for 6h to obtain colorless needle-shaped crystals. The chemical formula of the crystals was RbCd tested by XRD and ICP methods. 99.50% Mn 0.50% Cl3.
[0055] The crystal structures of the samples of Example 3 were tested respectively before heating (room temperature) and after heating (420K), and the samples were respectively denoted as RbCd 99.50% Mn0.50% Cl3- Room temperature and RbCd 99.50% Mn 0.50% Cl3-420K, it was found that the crystal structure was consistent with that of Example 1 under the same conditions, indicating that manganese doping did not affect its crystal structure.
[0056] Example 4
[0057] 0.3628g of rubidium chloride, 1.3749g of cadmium chloride and 1.4843g of manganese chloride tetrahydrate were put into 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for hydrothermal reaction and kept warm for 2h. Subsequently, the temperature was naturally lowered to room temperature, filtered, washed, and dried in an oven at 30℃ for 6h to obtain colorless needle-shaped crystals. The chemical formula was RbCd tested by XRD and ICP methods. 98.84% Mn 1.16% Cl3.
[0058] The crystal structures of the samples of Example 4 were tested respectively before heating (room temperature) and after heating (420K), and the samples were respectively denoted as RbCd 98.84% Mn 1.16% Cl3- Room temperature and RbCd 98.84% Mn 1.16% Cl3-420K, it was found that the crystal structure was consistent with that of Example 1 under the same conditions, indicating that manganese doping did not affect its crystal structure.
[0059] Example 5
[0060] 0.3628g of rubidium chloride, 1.0999g of cadmium chloride and 1.7812g of manganese chloride tetrahydrate were put into 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for hydrothermal reaction and kept warm for 2h. Subsequently, the temperature was naturally lowered to room temperature, filtered, washed, and dried in an oven at 30℃ for 6h to obtain colorless needle-shaped crystals. The chemical formula of the crystals was RbCd tested by XRD and ICP methods. 93.91% Mn 6.09% Cl3.
[0061] The crystal structures of the sample of Example 5 before and after heating (room temperature) and after heating (420K) were tested respectively, and the samples were denoted as RbCd 93.91% Mn 6.09% Cl3- Room temperature and RbCd 93.91% Mn 6.09% Cl3-420K, the results are shown in Figure 1 It was found that the crystal structure was consistent with that of Example 1 under the same conditions, indicating that manganese doping did not affect its crystal structure.
[0062] Comparative Example 1
[0063] 0.3628g of rubidium chloride, 0.8249g of cadmium chloride and 2.0781g of manganese chloride tetrahydrate were put into 15mL of concentrated hydrochloric acid to fully dissolve them, and then placed in a 50ml high-pressure reactor with a polytetrafluoroethylene liner. The high-pressure reactor was placed in an oven at 380K for hydrothermal reaction and kept warm for 2h. Subsequently, the temperature was naturally lowered to room temperature, filtered, washed, and dried in an oven at 30°C for 6h to obtain colorless needle-shaped crystals.
[0064] The crystal structure of the sample of comparative example 1 was tested without heating (room temperature), and the crystal structure of the sample was inconsistent with the crystal structure of example 1 under the same conditions.
[0065] The unheated (room temperature) sample was irradiated under ultraviolet light and observed, and no fluorescence phenomenon was observed. When the sample was heated to 420K, there was still no fluorescence phenomenon, indicating that the sample of Comparative Example 1 did not have thermochromic properties.
[0066] Test Example 1
[0067] RbCd 99.65% Mn 0.35% Cl3-room temperature, RbCd 99.50% Mn 0.50% Cl3-room temperature, RbCd 98.84% Mn 1.16% Cl3- Room temperature and RbCd 93.91% Mn 6.09% The fluorescence spectrum of Cl3- was tested at room temperature with an ultraviolet excitation wavelength of 245nm. Figure 2 It can be seen that under the excitation of ultraviolet light with a wavelength of 245nm, each sample exhibits red fluorescence of different intensities, and the fluorescence intensity increases with the increase of manganese doping. 93.91% Mn 6.09% The fluorescence intensity of Cl3- reaches the highest at room temperature.
[0068] RbCd 99.65% Mn 0.35% Cl3-420K、RbCd 99.50% Mn 0.50% Cl3-420K、RbCd 98.84% Mn 1.16% Cl3-420K and RbCd 93.91% Mn 6.09% Cl3-420K was used for fluorescence spectrum test, the UV excitation wavelength was 278nm, the results are shown in Figure 2 b. It can be seen that under the excitation of ultraviolet light with a wavelength of 278nm, each sample exhibits yellow fluorescence of different intensities. The fluorescence intensity increases with the increase of manganese doping.99.65% Mn 0.35% The fluorescence quantum efficiency of Cl3-420K is 71.79%, RbCd 93.91% Mn 6.09% The fluorescence intensity of Cl3-420K reaches the highest level, and its quantum efficiency can be as high as 100%.
[0069] Based on RbCd of Example 5 93.91% Mn 6.09% Cl3- Room temperature and RbCd 93.91% Mn 6.09% The fluorescence emission spectrum of Cl3-420K is plotted as a CIE diagram, and the results are shown in Figure 3 , from the chromaticity coordinate diagram, RbCd 93.91% Mn 6.09% Cl3- emits red light at room temperature, and its color coordinates are (0.609, 0.378). When the sample is heated to 420K, it emits yellow light and its color coordinates become (0.496, 0.450).
[0070] Test Example 3
[0071] The RbCd 93.91% Mn 6.09% Cl3- Room temperature and RbCd 93.91% Mn 6.09% Cl3-420K variable temperature fluorescence emission spectrum test. Test RbCd 93.91% Mn 6.09% The fluorescence of Cl3- at room temperature at test temperature from 160K to 480K, see Figure 4 In figure a, it can be seen that at 160K-420K, the fluorescence intensity increases with increasing temperature, and at 420K-480K, the fluorescence intensity decreases with increasing temperature, reaching a maximum at 420K. Test RbCd 93.91% Mn 6.09% The fluorescence of Cl3-420K at the test temperature from 300K to 480K. The results are shown in Figure 4 In middle b, the fluorescence intensity decreases as the temperature increases.
[0072] Test Example 4
[0073] Figure 5 In order to prepare the RbCd 93.91% Mn 6.09% The actual image of Cl3- room temperature at room temperature and heated to 420K and irradiated with 245nm ultraviolet lamp. 93.91% Mn 6.09%Cl3- emits red light at room temperature and under 245nm ultraviolet light, and turns into yellow light after being heated to 420K. When the sample temperature drops to room temperature again, it can still maintain yellow light emission when stored in air for 12 hours, and then gradually returns to red light emission. If it is sealed and stored (non-vacuum environment), it can maintain yellow light emission for at least 2 days, indicating that the sample of the present invention has obvious reversible thermochromic luminescence characteristics.
[0074] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes and modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes and modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A thermochromic luminescent material, characterized in that: The chemical formula of the thermochromic luminescent material is RbCd (1-x) Mn x Cl3; Wherein, x is the mole fraction, and its value range is 0<x≤15%.
2. The thermochromic luminescent material according to claim 1, characterized in that: At room temperature, RbCd (1-x) Mn x Cl3 belongs to the orthorhombic system, with a space group of Pnma. (1-x) Mn x When Cl3 is heated above 420K, its crystal structure changes to tetragonal and its space group changes to P4 / mbm.
3. The thermochromic luminescent material according to claim 1, characterized in that: At room temperature, when irradiated with ultraviolet light, the thermochromic luminescent material emits red light. When heated to above 420K, the thermochromic luminescent material emits yellow light.
4. The thermochromic luminescent material according to claim 1, characterized in that: The value range of x is 5-7%.
5. The method for preparing a thermochromic luminescent material according to any one of claims 1 to 4, characterized in that: The steps include: The rubidium-containing compound, the cadmium-containing compound and the manganese-containing compound are mixed, and then placed in a hydrogen chloride solution and heated until dissolved, and then the reaction solution is transferred to a hydrothermal reactor containing a polytetrafluoroethylene liner for hydrothermal reaction. After the reaction is completed, it is cooled, filtered and washed to obtain RbCd (1-x) Mn x Cl3 single crystal.
6. The preparation method according to claim 5, characterized in that: The rubidium-containing compound is selected from one or more of rubidium-containing oxides, rubidium-containing hydroxides, and rubidium-containing chlorides; The cadmium-containing compound is selected from one or more of cadmium-containing oxides, cadmium-containing hydroxides, and cadmium-containing chlorides; The manganese-containing compound is selected from one or more of manganese-containing oxides, manganese-containing hydroxides, and manganese-containing chlorides.
7. The preparation method according to claim 5, characterized in that: The temperature of the hydrothermal reaction is 360-400K, and the time of the hydrothermal reaction is 2-8h.
8. Application of the thermochromic luminescent material according to any one of claims 1 to 4 in intelligent response luminescence, anti-counterfeiting and temperature detection.
9. Anti-counterfeiting material, characterized in that: The invention comprises the thermochromic luminescent material according to any one of claims 1 to 4.
10. The temperature detection device is characterized in that: The invention comprises the thermochromic luminescent material according to any one of claims 1 to 4.
Citation Information
Patent Citations
Metal halide perovskite luminescent material capable of efficiently emitting yellow light and resisting thermal quenching as well as preparation method and application of metal halide perovskite luminescent material
CN116355612A
Antimony-doped bismuth-based chlorine compound as well as preparation and application thereof
CN117467440A