Method for hydrothermal carbonization of DES catalyzed biogas residues and saw dust

By synergistically catalyzing biogas residue and garden waste with DES catalyst, the problems of high energy consumption and low catalyst efficiency in hydrothermal carbonization technology are solved, an efficient and environmentally friendly hydrothermal carbonization process is realized, biochar with high calorific value is prepared, and the problem is solved Difficulties in preparing traditional coal replacement products.

CN118725930APending Publication Date: 2024-10-01JIANGSU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410715777.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hydrothermal carbonization technology has problems such as high energy consumption, low catalyst efficiency, and pollution caused by the use of catalysts. It is difficult to effectively utilize kitchen digestate and garden waste to prepare traditional coal replacement products with high calorific value.

Method used

DES catalyst is used to synergistically catalyze the hydrothermal carbonization of biogas residue and garden waste. Through mechanical crushing, deionized water addition, deoxidation heating and drying steps, the temperature and energy consumption are reduced, and the use of traditional catalysts is avoided. Choline chloride is used with A mixture of ethylene glycol, urea, and oxalic acid serves as a catalyst.

Benefits of technology

It achieves efficient hydrothermal carbonization at lower temperatures, saves energy, reduces carbon emissions, and prepares biochar with high calorific value. The process is environmentally friendly, has no discharge of waste water and exhaust gas, and reduces the use of catalysts and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725930A_ABST
    Figure CN118725930A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid waste resource utilization, and relates to a hydrothermal carbonization method for synergy of DES catalysis biogas residues and saw dust, in particular to a method for preparing high-calorific-value hydrothermal carbon through hydrothermal carbonization of kitchen waste fermentation biogas residues and garden waste. The preparation method comprises the following steps: mixing kitchen biogas residues, garden wastes, water and the like according to a certain proportion, adding a DES catalyst under the conditions of certain temperature, pressure and time, carrying out a hydrothermal carbonization reaction, and after the reaction is finished, cooling, filtering and drying a solid product to obtain the hydrothermal carbon. The hydrothermal carbon prepared by the method has the characteristics of high calorific value, low ash content and the like, can be used as an effective substitute of traditional fire coal, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste resource utilization and relates to a method for hydrothermal carbonization of biogas residue catalyzed by DES and coordinated with sawdust. Background Art

[0002] Since food digestate contains a lot of organic components and garden waste contains a lot of cellulose, hemicellulose, lignin, etc., these urban organic solid wastes have high potential calorific value and can be used to make fuel, thus achieving the purpose of waste resource utilization.

[0003] Among the many carbon-containing biomass treatment technologies, hydrothermal carbonization is an efficient and effective resource-based treatment technology. This technology is to place biomass with a high moisture content or mix water and dry biomass in a certain proportion in a reactor, and perform hydrothermal reaction under a certain temperature, pressure, reaction time and catalyst to convert biomass into a series of high value-added products mainly composed of hydrothermal carbon. The hydrothermal carbonization of biogas residues, garden waste, etc. is a process of heating and pressurizing biogas residues, garden waste, etc. to break down the cells in these raw materials into small molecules, and generate organic carbon through a series of reactions such as hydrolysis, dehydration, decarboxylation, condensation and aromatization. The advantage of hydrothermal carbonization of biogas residues and garden waste is that hydrothermal carbonization removes water from these raw materials and generates small molecules by cracking, with low energy consumption, high carbon content in the generated products, and high calorific value. Biogas residues, garden waste, etc. that have been treated with hydrothermal carbonization can be processed into various biomass fuels for power generation in power plants, heat generation in boilers, or as civil fuels.

[0004] However, the current hydrothermal carbonization technology has problems such as high energy consumption, low catalyst efficiency and pollution caused by the use of catalysts. If the technical problems in the above process can be solved, using biogas residues, garden waste and other materials as the main raw materials to produce alternative products for traditional coal, as zero-carbon or carbon-negative materials, it will play an important role in energy conservation and emission reduction, environmental protection and achieving dual carbon goals. Summary of the invention

[0005] The purpose of the present invention is to overcome some technical problems existing in the prior art and to provide a method for efficiently catalyzing the hydrothermal carbonization of kitchen waste and garden waste and preparing high calorific value hydrothermal carbon.

[0006] To achieve the above object, the present invention provides a method for hydrothermal carbonization of biogas residue catalyzed by DES and coordinated with garden waste, the method comprising the following steps:

[0007] The biogas residue and garden waste are mechanically crushed respectively, passed through a 60-mesh sieve, and stored for later use; the pretreated biogas residue and garden waste are weighed respectively according to a certain mass ratio, and deionized water is added to the reaction system and stirred evenly; DES catalyst is added, the reaction system is deoxygenated and then heated to react, and the solid and liquid products are separated after cooling to room temperature, and the solid product is dried to obtain hydrothermal charcoal.

[0008] Among them, the biogas residue is obtained by fermenting food waste, and the garden waste includes pine sawdust; the mass ratio of the biogas residue to the garden waste is 3-7:7-3, preferably, the mass ratio of the biogas residue to the garden waste is 3:7; the amount of deionized water is added at a solid-liquid ratio of 1:9.

[0009] Further preferably, the biogas residue has a water content of 8.6%, and the garden waste has a water content of 12.1%.

[0010] The amount of the DES catalyst added is 10% of the total mass of the reaction system; the DES catalyst comprises a mixture of choline chloride with ethylene glycol, urea and oxalic acid in different molar ratios, wherein the molar ratio of choline chloride to ethylene glycol, urea and oxalic acid is 1:1-2, preferably, the molar ratio of choline chloride to ethylene glycol is 1:2, the molar ratio of choline chloride to urea is 1:2, and the molar ratio of choline chloride to oxalic acid is 1:1.

[0011] The deoxygenation of the reaction system is performed by replacing the reaction system with N2 for 3-5 times.

[0012] The temperature of the temperature-raising reaction is 200-250° C., and the reaction time is 30-60 min. Preferably, the temperature of the temperature-raising reaction is 250° C., and the reaction time is 30 min.

[0013] The drying was carried out at 105°C for 72 hours.

[0014] The ash content of the hydrothermal charcoal obtained is measured by a muffle furnace, the ash temperature is 850° C., and the time is 60 min; the calorific value of the hydrothermal charcoal obtained is measured by a fully automatic calorimeter.

[0015] The invention also provides hydrothermal charcoal prepared by the method.

[0016] The beneficial effects of the present invention are as follows:

[0017] (1) The method of the present invention cooperates with biogas residue and garden waste to achieve reasonable and efficient utilization of both kitchen biogas residue and garden waste through a hydrothermal carbonization process, thereby effectively utilizing waste resources, realizing the resource utilization of wastes such as kitchen waste and garden waste, greatly reducing carbon emissions, and at the same time, producing biochar of relatively good quality.

[0018] (2) The method of the present invention can perform hydrothermal carbonization at a lower temperature, which is more energy-saving than conventional carbonization processes. The preparation method provided by the present invention can achieve no discharge of wastewater and waste gas, and no solid waste is generated.

[0019] (3) The method of the present invention avoids the use of traditional catalysts for hydrothermal carbonization, such as acid, alkali, metal ions, etc., and uses DES as a catalyst to make the hydrothermal carbonization process more economical, environmentally friendly and efficient.

[0020] Deep eutectic solvent (DES) is essentially an ion mixture, which not only has the characteristics of low volatility, low melting point, thermal stability, good solubility, designability and the like of ionic liquids, but also has the good properties of simple synthesis and biodegradability. At present, the method of preparing DES using choline chloride and using it as a solvent for the pretreatment of lignocellulose has the problems of large amount of solvent and high cost, and it is difficult to achieve large-scale application. In the method of the present invention, choline chloride is used as a hydrogen bond acceptor, and different hydrogen bond donors are used to prepare acidic, alkaline and neutral DES respectively, and use them as catalysts for multi-component reaction systems, not only the amount of DES used is small, but DES can also dissolve part of organic matter, realizing the multi-purpose utilization of DES. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the hydrothermal carbonization process of the present invention.

[0022] Figure 2 This is the hydrothermal carbonization effect diagram when the ratio of sludge to sawdust is 3:7 under the action of different DES catalysts. DETAILED DESCRIPTION

[0023] In order to make the purpose, features and advantages of the present invention more obvious and understandable, the embodiments of the present invention are clearly and completely described below in conjunction with the specific implementation methods involved in the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work, such as embodiments that only change the purpose without changing the basic principles involved in the claims, belong to the scope of protection of the present invention.

[0024] The biogas residue involved in the present invention is obtained by fermenting kitchen waste, and the fermentation method is not limited.

[0025] The present invention is further described below in conjunction with specific embodiments.

[0026] Embodiment 1:

[0027] This embodiment provides a method for hydrothermal carbonization of biogas residue catalyzed by DES and coordinated with sawdust, comprising the following steps:

[0028] The kitchen digestate (containing 8.6% water) and pine sawdust (containing 12.1% water) were respectively ground, passed through a 60-mesh sieve, and stored for later use; the ground kitchen digestate and pine sawdust were mixed in a mass ratio of 3:7 and added to a reactor; deionized water and a DES catalyst (a mixture of choline chloride and oxalic acid in a molar ratio of 1:1) accounting for 10% of the mass of the reaction system were added in a solid-liquid ratio of 1:9; the gas in the reactor system was replaced with N2 three times to ensure that the reaction system was in an inert gas atmosphere; the reactor was heated to a set temperature of 250°C, and the reactant system was kept warm for 30 minutes; after the insulation was completed, it was naturally cooled to room temperature; the reactor was opened and the hydrothermal carbonization reaction product was taken out; the reaction product was filtered, the solid product was taken, and the liquid was used for other purposes; the solid product was dried at 105°C for 72 hours to obtain hydrothermal carbonization.

[0029] The ash content of the hydrothermal charcoal was determined using a muffle furnace, with the ashing temperature set at 850°C and the time set at 60 min. The calorific value of the hydrothermal charcoal was determined using a fully automatic calorimeter, and the high calorific value was selected.

[0030] In the present invention, based on Example 1, other conditions remain unchanged, and the conditions for heating the reactor are adjusted. When the temperature is set to 200°C, the reactant system is kept warm for 30 minutes, and the calorific value of the prepared hydrothermal carbon is 4797.75 kcal and the ash content is 23.65%; when the temperature is set to 250°C, the reactant system is kept warm for 60 minutes, and the calorific value of the prepared hydrothermal carbon is 5016.15 kcal and the ash content is 21.95%. Combined with the results of Examples 1-3, the present invention preferably prepares under the conditions of 250°C and 30 minutes.

[0031] Embodiment 2:

[0032] This embodiment provides a method for hydrothermal carbonization of biogas residue catalyzed by DES and coordinated with sawdust, comprising the following steps:

[0033] The kitchen digestate (containing 8.6% water) and pine sawdust (containing 12.1% water) were respectively ground, passed through a 60-mesh sieve, and stored for later use; the ground kitchen digestate and pine sawdust were mixed in a ratio of 3:7 and added into a reactor; deionized water and a DES catalyst (a mixture of choline chloride and ethylene glycol in a molar ratio of 1:2) accounting for 10% of the mass of the reaction system were added in a solid-liquid ratio of 1:9; the gas in the reactor system was replaced with N2 for 3 times; the reactor was heated to a set temperature of 250°C, and the reactant system was kept warm for 30 minutes; after the insulation was completed, the system was naturally cooled to room temperature; the reactor was opened and the hydrothermal carbonization reaction product was taken out; the reaction product was filtered, the solid product was taken, and the liquid was used for other purposes; the solid product was dried at 105°C for 72 hours to obtain hydrothermal carbonization.

[0034] The ash content of the hydrothermal charcoal was determined using a muffle furnace, with the ashing temperature set at 850°C and the time set at 60 min. The calorific value of the hydrothermal charcoal was determined using a fully automatic calorimeter, and the high calorific value was selected.

[0035] Embodiment 3:

[0036] This embodiment provides a method for hydrothermal carbonization of biogas residue catalyzed by DES and coordinated with sawdust, comprising the following steps:

[0037] The kitchen digestate (containing 8.6% water) and pine sawdust (containing 12.1% water) were respectively ground, passed through a 60-mesh sieve, and stored for later use; the ground kitchen digestate and pine sawdust were mixed in a ratio of 3:7 and added into a reactor; deionized water and a DES catalyst (a mixture of choline chloride and urea in a molar ratio of 1:2) accounting for 10% of the reaction system mass were added in a solid-liquid ratio of 1:9; the reactor system was gas replaced with N2 for 3 times; the reactor was heated to a set temperature of 250°C, and the reactant system was kept warm for 30 minutes; after the insulation was completed, the system was naturally cooled to room temperature; the reactor was opened and the hydrothermal carbonization reaction product was taken out; the reaction product was filtered, the solid product was taken, and the liquid was used for other purposes; the solid product was dried at 105°C for 72 hours to obtain hydrothermal carbonization.

[0038] The ash content of the hydrothermal charcoal was determined using a muffle furnace, with the ashing temperature set at 850°C and the time set at 60 min. The calorific value of the hydrothermal charcoal was determined using a fully automatic calorimeter, and the high calorific value was selected.

[0039] In these embodiments, different types of DES were used as catalysts, and the calorific value and ash content of the obtained hydrothermal carbon were also different, as shown in Table 1. Therefore, in practical applications, different types of DES catalysts are selected according to the properties of different reactant systems to achieve the best hydrothermal carbonization effect.

[0040] Table 1. Hydrothermal carbonization effect of biogas residue and sawdust with different DES catalysts

[0041]

[0042] As can be seen in Table 1, through 3 parallel experiments, the average value was calculated. The results show that the introduction of DES catalyst in the method of the present invention can greatly improve the hydrothermal carbonization effect, the calorific value is greatly improved, and the ash content is reduced. It can be seen that the method of the present invention coordinates the application of biogas residue and garden waste, and after adding DES catalyst, the hydrothermal carbon obtained has a better effect.

[0043] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for hydrothermal carbonization of biogas residues catalyzed by DES and garden waste. It is characterized in that The method comprises the following steps: The biogas residue and garden waste are mechanically crushed respectively, sieved and stored for later use; the pretreated biogas residue and garden waste are weighed respectively according to a certain mass ratio, and deionized water is added to the reaction system and stirred evenly; DES catalyst is added, the reaction system is deoxygenated and heated to react, and the solid and liquid products are separated after cooling to room temperature, and the solid product is dried to obtain hydrothermal charcoal.

2. The method according to claim 1, It is characterized in that The biogas residue is obtained by fermenting kitchen waste, and the garden waste includes pine sawdust; the mass ratio of the biogas residue to the garden waste is 3-7:7-3, preferably, the mass ratio of the biogas residue to the garden waste is 3:7; the deionized water is added at a solid-liquid ratio of 1:

9.

3. The method according to claim 1, It is characterized in that The amount of the DES catalyst added is 10% of the total mass of the reaction system; the DES catalyst comprises a mixture of choline chloride with ethylene glycol, urea and oxalic acid in different molar ratios, wherein the molar ratio of choline chloride to ethylene glycol, urea and oxalic acid is 1:1-2.

4. The method according to claim 3, It is characterized in that The molar ratio of choline chloride to ethylene glycol is 1:2, the molar ratio of choline chloride to urea is 1:2, and the molar ratio of choline chloride to oxalic acid is 1:

1.

5. The method according to claim 1, It is characterized in that The reaction system is deoxygenated by using N 2 Replace 3-5 times.

6. The method according to claim 1, It is characterized in that The temperature of the temperature-raising reaction is 200-250° C., and the reaction time is 30-60 min.

7. The method according to claim 6, It is characterized in that The temperature of the temperature-raising reaction is 250° C., and the reaction time is 30 min.

8. The method according to claim 1, It is characterized in that The drying was carried out at 105°C for 72 hours.

9. The method according to claim 1, It is characterized in that The ash content of the obtained hydrothermal char was measured, and the ash temperature was 850°C.

10. Hydrothermal charcoal prepared according to the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • A method for directional preparation of sludge solvothermal carbon by using a deep eutectic solvent