Bio-based modified graphene as well as preparation method and application thereof

Through the preparation of bio-based modified graphene, bio-based fatty acid esters and polyamine compounds are used to react with graphene oxide to form modified groups with high grafting rates, which improves the dispersion stability and metal surface affinity of graphene. It solves the problems of insufficient anti-wear performance and corrosion in the existing technology, and achieves long-lasting lubrication and anti-wear effects.

CN118725933APending Publication Date: 2024-10-01NINGBO GRAPHENE INNOVATION CENT CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410713611.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the prior art, the anti-wear performance of graphene in lubricants still needs to be improved, and it is prone to corrosion on metal surfaces.

Method used

By reacting bio-based fatty acid esters with graphene oxide and polyamine compounds, bio-based modified graphene is formed, which improves its dispersion stability in bio-based base oil and forms a high-strength surface film through pyrolysis reaction. Improve anti-wear performance while avoiding corrosion.

Benefits of technology

It achieves the long-term lubrication performance and extreme pressure anti-wear effect of graphene, extends the service life of the anti-wear agent, reduces the wear of machine parts, and does not contain moisture and heavy metal impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725933A_ABST
    Figure CN118725933A_ABST
Patent Text Reader

Abstract

The invention discloses bio-based modified graphene as well as a preparation method and application thereof. The bio-based modified graphene comprises graphene, a linking group and a modification group which are sequentially connected, the modification group comprises a bio-based fatty acid group, the linking group is derived from a polyamine compound, and different amino groups react with epoxy groups and / or carboxyl groups on the surface of graphene oxide respectively to form connection with graphene. And reacting with a bio-based fatty acid ester to form a connection with a modification group. The preparation method comprises the following steps: enabling graphene oxide, bio-based fatty acid ester and a polyamine compound to form a modified reaction system; and reacting to obtain the bio-based modified graphene. The bio-based modified graphene provided by the invention is grafted and modified by the bio-based fatty acid ester through the polyamine compound, so that the bio-based modified graphene has excellent long-term effect; the metal surface affinity is excellent, and the anti-attrition onset time can be remarkably shortened; and the anti-wear agent has the characteristic of no corrosion, and can reduce the abrasion of machine parts and prolong the service life of the anti-wear agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of anti-wear agents, and in particular to bio-based modified graphene, a preparation method and application thereof. Background Art

[0002] Bio-based base oils are made from bio-based raw materials, which are renewable and sustainable. Compared with traditional mineral base oils, bio-based base oils have less emissions, better biodegradability, higher lubricity, lower activity, better skin compatibility, higher viscosity index and better safety.

[0003] As a new type of nanomaterial, graphene has the advantages of excellent mechanical anti-wear performance, chemical stability and biocompatibility, and is an important friction modifier and extreme pressure agent. Graphene is dispersed in various lubricants, so that the lubricated parts are in a relaxed working condition, and a physical and adsorbable interface with friction reduction and anti-wear effects is formed on the friction surface to quickly form an oil film, achieving the effect of lubrication and friction reduction. Graphene not only has excellent friction reduction and anti-wear performance, but also has good extreme pressure anti-wear and oxidation resistance, and has good application prospects in lubricants such as internal combustion engine oil and grease.

[0004] Antiwear agent is a lubricant additive that can reduce engine wear and increase engine power. It is also called engine maintenance agent or powerful repair agent. It can extend the service life of engine oil, save fuel and increase power. The respective characteristics of bio-based base oil and graphene determine that they have broad application prospects in the field of antiwear agents.

[0005] However, in the prior art, when graphene is modified with flexible segments and dispersed in lubricants for anti-wear lubrication applications, the anti-wear performance still needs to be improved and corrosion of the metal surface is likely to occur. Summary of the invention

[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide a bio-based modified graphene, a preparation method and application thereof.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0008] In a first aspect, the present invention provides a bio-based modified graphene, which includes graphene, a connecting group and a modifying group connected in sequence, wherein the modifying group includes a bio-based fatty acid group, the connecting group is derived from a polyamine compound, and different amine groups of the polyamine compound react with epoxy groups and / or carboxyl groups on the surface of graphene oxide to form a connection with the graphene, and react with bio-based fatty acid esters to form a connection with the modifying group.

[0009] In a second aspect, the present invention further provides a method for preparing the above-mentioned bio-based modified graphene, which comprises:

[0010] Fully mixing graphene oxide, bio-based base oil, and polyamine compound to form a modified reaction system, wherein the bio-based base oil is bio-based fatty acid ester;

[0011] The modified reaction system is reacted to obtain bio-based modified graphene.

[0012] In a third aspect, the present invention also provides a graphene bio-based anti-wear agent, which includes a bio-based base oil, a paraffin-based base oil, the above-mentioned bio-based modified graphene and selected additives.

[0013] In a fourth aspect, the present invention also provides the use of the above-mentioned graphene bio-based anti-wear agent in metal surface lubrication, more specifically as an engine oil additive.

[0014] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include:

[0015] 1. The bio-based modified graphene provided by the present invention is grafted and modified by bio-based fatty acid esters through polyamine compounds, which can not only improve the grafting rate and thus increase the number of modified groups, but also make its surface energy close to the surface energy of the bio-based base oil itself, so that it can be dispersed stably in the bio-based base oil for a long time. At the same time, the dispersion effect is further improved under the action of the dispersant, so that the anti-wear agent can give full play to the lubricating properties of the graphene and have excellent long-term effectiveness.

[0016] 2. In the present invention, graphene is grafted and modified to greatly improve its affinity to the metal surface. The anti-wear agent is coated on the friction metal surface. At the moment when the friction metal surface is subjected to high-speed running-in, the bio-based modified graphene undergoes a pyrolysis reaction, and the surface grafted groups partially fall off, and then firmly adhere to the metal surface, forming a surface film with excellent lubrication properties and extremely high strength, which plays an extreme pressure, anti-wear and wear-reducing role.

[0017] 3. The bio-based anti-wear agent provided by the present invention is non-corrosive, does not contain water and heavy metal impurities, has good lubricity, can reduce the wear of machine parts, and prolong the service life of the anti-wear agent. The excellent metal affinity of the bio-based base oil can promote the rapid formation of an oil film between graphene and lubricating oil. The surface oil film is adsorbed on the metal surface to play the role of extreme pressure, anti-wear, wear reduction and repair.

[0018] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a test curve diagram of the friction coefficient of lubricating oil provided by some typical implementation cases and comparative cases of the present invention;

[0020] Figure 2a This is a photo of the wear spot test of the blank sample provided by the present invention;

[0021] Figure 2b This is a photo of the wear spot test of Example 4 provided by the present invention;

[0022] Figure 2c This is a photo of the wear spot test of Comparative Example 2 provided by the present invention. DETAILED DESCRIPTION

[0023] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0024] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0025] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component or method step from another with the same name, but do not necessarily require or imply any such actual relationship or order between these components or method steps.

[0026] An embodiment of the present invention provides a bio-based modified graphene, whose microstructure includes graphene, a connecting group and a modifying group connected in sequence, wherein the modifying group includes a bio-based fatty acid group, the connecting group is derived from a polyamine compound, and different amine groups of the polyamine compound react with epoxy groups and / or carboxyl groups on the surface of graphene oxide to form a connection with the graphene, and react with bio-based fatty acid esters to form a connection with the modifying group.

[0027] Of course, the above structure is the group composition and connection relationship with significant characteristics provided by the present invention, but it is not all the structural characteristics. In addition, the bio-based modified graphene can also be connected by an ester exchange reaction between the bio-based fatty acid ester and the hydroxyl group of the graphene itself.

[0028] The prior art provides a variety of technical solutions for modifying the lipophilicity of graphene by grafting long fatty chain segments onto the graphene surface. For example, some prior arts use silane coupling agents to graft fatty alkylamines onto the graphene surface, and other prior arts use higher fatty alcohols to directly react with carboxyl groups on the surface of graphene oxide to cause fatty chains to connect to the graphene surface.

[0029] However, in the above-mentioned prior art, the grafting rate on the graphene surface is still not ideal, which leads to room for improvement in its dispersion capacity and dispersion stability when used as an antiwear agent; and in order to improve the dispersion stability of graphene in bio-based base oil, the present invention considers using bio-based base oil (i.e., bio-based fatty acid ester, which is a mixture of multiple fatty acid esters) to modify graphene oxide to obtain bio-based modified graphene, and the bio-based fatty acid ester can undergo ester exchange reaction with the hydroxyl group on the graphene oxide to achieve grafting; the bio-based fatty acid ester cannot react with the epoxy group or carboxyl group on the graphene oxide. In order to improve the grafting rate, the present invention preferably adds a polyamine substance as a bridging group, and the amino group can react with the carboxyl group and epoxy group on the graphene oxide, and can also react with fatty acid methyl ester, thereby realizing the connection between the carboxyl group and epoxy group on the graphene oxide and the fatty acid methyl ester, significantly improving the grafting rate, thereby achieving the effect of enhancing the dispersion effect.

[0030] The bio-based mentioned here refers to bio-based base oil. Generally speaking, bio-based base oil comes from biodiesel (commercially available product). Biodiesel can be distilled to obtain the fraction in a specific boiling point range to obtain bio-based base oil. The main component of bio-based base oil is fatty acid methyl ester (or ethyl ester).

[0031] As some typical examples, bio-based fatty acid esters can be components with a boiling point above 300°C in commercially available biodiesel, such as fractions above 300°C collected by distillation. Of course, it is not excluded to use other technical means to obtain bio-based fatty acid esters with the same molecular characteristics as the above-mentioned bio-based base oil, or to adjust the preparation conditions (for example, the distillation temperature may be adjusted under different pressures, etc.) to obtain bio-based base oils with similar component characteristics. All feasible equivalent implementation means belong to the protection scope of the present invention.

[0032] In addition, in addition to the above-mentioned method of preparing the bio-based base oil by commercially available bio-based diesel, in some other typical examples, the following method can be used to prepare the bio-based base oil containing the bio-based fatty acid ester:

[0033] Bio-based raw materials (animal and plant oils, triglycerides) are subjected to ester exchange reaction with methanol (methanol, ethanol, propanol, isopropanol and other lower alcohols) under the catalysis of concentrated sulfuric acid, the reaction temperature is 70℃-90℃, and the reaction time is 5-6h. After the crude ester is cooled and left to stand for 12 hours, the lower layer of dilute sulfuric acid and glycerol water are released. Saturated salt water containing 10% (8%-15%) soda ash is added to the crude ester for neutralization reaction to obtain water-washed crude ester, and then industrial soda ash is added to the water-washed crude ester and heated for distillation. Only the fractions above 300℃ (280℃-350℃) are collected to obtain bio-based fatty acid esters.

[0034] As for the specific group selection, in some embodiments, the polyamine compound includes any one or a combination of two or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, aminoethylpiperazine, polyetheramine, and hydroxyethylethylenediamine;

[0035] In some embodiments, the bio-based fatty acid ester includes a fatty acid ester formed by a bio-based fatty acid and a lower alcohol;

[0036] In some embodiments, the lower alcohol includes any one of methanol, ethanol, propanol, isopropanol, or a combination of two or more thereof.

[0037] This means that how to obtain the bio-based base oil is not a key step of the present invention. In this article, the extraction method involved in the specific embodiment is only for exemplary purposes.

[0038] The animal oils include lard, beef tallow, mutton fat, horse oil, chicken fat, duck fat, goose fat, etc.; the vegetable oils include soybean oil, palm oil, rapeseed oil, sunflower oil, corn oil, cottonseed oil, coconut oil, etc.; in order to further reduce costs, even recycled cooking oil can be used.

[0039] In order to obtain the above material, the embodiment of the present invention also provides a method for preparing the above bio-based modified graphene, which comprises the following steps:

[0040] Fully mixing graphene oxide, bio-based base oil, and polyamine compound to form a modified reaction system, wherein the bio-based base oil is bio-based fatty acid ester;

[0041] The modified reaction system is reacted to obtain bio-based modified graphene.

[0042] Specifically, different amine groups in the polyamine compound react with the epoxy group and / or carboxyl group on the surface of the graphene oxide, and react with the bio-based fatty acid ester to form an amide group, thereby obtaining bio-based modified graphene. Of course, there is also a case where the bio-based fatty acid ester directly undergoes an ester exchange reaction with the hydroxyl group on the surface of the graphene oxide and is directly connected.

[0043] In some embodiments, in the modification reaction system, the amount of the graphene oxide added is 1 part by mass, the amount of the bio-based base oil added is 10-50 parts by mass, and the amount of the polyamine compound added is 1-5 parts by mass.

[0044] In some embodiments, the modified reaction system further contains a first dispersant;

[0045] In some embodiments, the first dispersant includes any one or a combination of two or more of polyvinyl pyrrolidone, polymethacrylate, ethylene propylene copolymer, polyisobutylene, and hydrogenated styrene diene copolymer;

[0046] In some embodiments, based on 1 part by mass of the graphene oxide, the added amount of the first dispersant is 0.1-0.5 parts by mass.

[0047] In some embodiments, the preparation method may specifically include:

[0048] The modified reaction system is heated and emulsified under vacuum conditions, the heating temperature is 80-140° C., the emulsification speed is 8000-14000 rpm, and the reaction time is 4-8 hours;

[0049] The product obtained after the reaction is completed is dried to obtain the bio-based modified graphene.

[0050] Ultrasonic treatment makes the graphene dispersion more uniform and stable, and vacuuming can reduce the reaction temperature and accelerate the reaction.

[0051] As some typical application examples of the above technical solution, the above preparation method can be implemented by the following specific steps:

[0052] Add a slurry containing 1 part of graphene oxide to 10-50 parts of bio-based base oil, stir evenly, add 1-5 parts of polyamine substances (ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, polyetheramine, hydroxyethylethylenediamine), add a dispersant (polyvinylpyrrolidone PVP), heat to 80-140°C, react for 4-8 hours, evacuate during the reaction, and perform ultrasonic treatment (300W-1000W) at the same time. After the reaction is completed, dry in a vacuum oven at 100°C for 24 hours to obtain bio-based modified graphene.

[0053] As a further application of the above technical solution, an embodiment of the present invention further provides a graphene bio-based anti-wear agent, which includes a bio-based base oil, a paraffin-based base oil, a bio-based modified graphene provided or prepared by any of the above embodiments, and a selected additive.

[0054] In some embodiments, the graphene bio-based anti-wear agent comprises, by weight, 5-10 parts of bio-based modified graphene, 20-40 parts of bio-based base oil, and 40-60 parts of paraffin base oil.

[0055] In some embodiments, the selected additives include antioxidants, rust inhibitors, and second dispersants;

[0056] In some embodiments, the graphene bio-based anti-wear agent comprises 1-3 parts of an antioxidant, 1-3 parts of a rust inhibitor, and 3-5 parts of a second dispersant, by weight;

[0057] In some embodiments, the antioxidant includes any one of alkylphenol zinc salt, butyl octyl zinc salt, and dioctyl basic zinc salt, or a combination of two or more thereof; the rust inhibitor includes any one of heavy alkylbenzene sulfonate barium, petroleum sulfonate barium, basic dinonylnaphthalene sulfonate barium, and dodecenylsuccinic acid, or a combination of two or more thereof; and the second dispersant includes any one of polyisobutylene amine, polyisobutylene succinimide, polyisobutylene succinic anhydride, polyether amine, and Span 80, or a combination of two or more thereof.

[0058] As some typical application examples of the above technical solution, the above anti-wear agent includes, by mass, 5 to 10 parts of bio-based modified graphene, 20 to 40 parts of bio-based base oil, 1 to 3 parts of antioxidant (sulfur alkylphenol zinc salt, sulfur butyl octyl zinc salt, sulfur bisoctyl basic zinc salt), 1 to 3 parts of rust inhibitor (heavy alkylbenzene sulfonate barium, petroleum sulfonate barium, basic dinonylnaphthalene sulfonate barium, dodecenylsuccinic acid, etc.), 3 to 5 parts of dispersant (polyisobutylene succinimide), and 40 to 60 parts of base oil (paraffin-based oil).

[0059] The preparation method of the anti-wear agent specifically comprises: putting 5-10 parts of the above-mentioned bio-based modified graphene, 20-40 parts of bio-based base oil, 1-3 parts of antioxidant, 1-3 parts of rust inhibitor, 3-5 parts of dispersant and 40-60 parts of base oil into a reaction kettle, stirring at a high speed (1000-2000 rpm) for 3-7 hours at a temperature of 65°C-85°C to obtain a graphene bio-based anti-wear agent.

[0060] Furthermore, an embodiment of the present invention also provides the use of the graphene bio-based anti-wear agent provided by any of the above-mentioned embodiments in metal surface lubrication.

[0061] In particular, the graphene bio-based anti-wear agent provided by the present invention is used as an engine oil additive.

[0062] The technical solution of the present invention is further described in detail below through several embodiments. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.

[0063] Example 1

[0064] This example illustrates the preparation process of the bio-based base oil (also the bio-based fatty acid ester used in Example 2), as shown below:

[0065] Take commercially available biodiesel (a mixture of various fatty acid methyl esters or ethyl esters), heat and distill it, collect the fractions above 300°C, and obtain bio-based base oil.

[0066] It should be noted that this embodiment illustrates a process for obtaining a bio-based base oil, but the bio-based base oil that can be selected in the present invention is not limited to the product provided in this embodiment. Products prepared by other methods or with similar components available on the market can still achieve equivalent effects and meet the core technical concept provided by the present invention.

[0067] Example 2

[0068] This embodiment illustrates the preparation process of bio-based modified graphene, which is specifically as follows:

[0069] Add a graphene oxide aqueous dispersion containing 1 part of graphene oxide to 20 parts of bio-based base oil, stir evenly, add 2 parts of polyethylene polyamine (a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, etc., which can be obtained commercially) and a dispersant (polyvinyl pyrrolidone PVP, added in an amount of 0.3 parts) and heat to 120°C, react for 6 hours, evacuate during the reaction, and stir at a high speed of 8000 rpm. After the reaction is completed, dry in a vacuum oven at 100°C for 24 hours to obtain bio-based modified graphene 1#.

[0070] Example 3

[0071] This embodiment illustrates the preparation process of graphene bio-based anti-wear agent, which is specifically as follows:

[0072] The graphene bio-based anti-wear agent is prepared by using 5 parts of bio-based modified graphene 1#, 1 part of sulfur phosphorus alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 40 parts of bio-based base oil, 3 parts of polyisobutylene succinimide and 45 parts of paraffin-based base oil, based on mass.

[0073] Embodiment 4:

[0074] This embodiment illustrates the preparation process of another ratio of graphene bio-based anti-wear agent, which is specifically as follows:

[0075] The graphene bio-based anti-wear agent is prepared by using 10 parts of bio-based modified graphene 1#, 1 part of sulfur phosphorus alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 40 parts of bio-based base oil, 3 parts of polyisobutylene succinimide and 40 parts of paraffin-based base oil, based on mass.

[0076] Comparative Example 1

[0077] This comparative example illustrates the formulation of a control antiwear agent, which is substantially the same as Example 3, except that the addition of bio-based modified graphene is omitted, and the omitted bio-based modification is replaced by an equal amount of paraffin-based base oil:

[0078] The bio-based anti-wear agent is prepared from 1 part of alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 40 parts of bio-based base oil, 3 parts of polyisobutylene succinimide and 50 parts of paraffin-based base oil, based on mass.

[0079] Comparative Example 2

[0080] This comparative example illustrates the formulation of a control antiwear agent, which is substantially the same as Example 4, except that the addition of the bio-based base oil is omitted, and the omitted bio-based base oil is replaced with an equal amount of paraffin-based base oil:

[0081] Calculated by mass, 10 parts of bio-based modified graphene 1#, 1 part of sulfur phosphorus alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 3 parts of polyisobutylene succinimide and 80 parts of paraffin-based base oil are used to prepare a graphene anti-wear agent.

[0082] Comparative Example 3

[0083] This comparative example is substantially the same as Example 2-3, except that methyl oleate is used to replace the bio-based base oil:

[0084] Add a graphene oxide aqueous dispersion containing 1 part of graphene oxide to 20 parts of methyl oleate, stir evenly, add 2 parts of polyethylene polyamine and a dispersant (polyvinyl pyrrolidone PVP, added in an amount of 0.3 parts), heat to 120°C, react for 6 hours, evacuate during the reaction, and stir at a high speed of 8000 rpm. After the reaction is completed, dry in a vacuum oven at 100°C for 24 hours to obtain bio-based modified graphene 2#.

[0085] The graphene bio-based anti-wear agent is prepared by using 5 parts of bio-based modified graphene 2#, 1 part of sulfur phosphorus alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 40 parts of bio-based base oil, 3 parts of polyisobutylene succinimide and 45 parts of paraffin-based base oil, based on mass.

[0086] Comparative Example 4

[0087] This comparative example is substantially the same as Example 2-3, except that no polyamines are added:

[0088] Add a graphene oxide aqueous dispersion containing 1 part of graphene oxide to 20 parts of bio-based base oil, add a dispersant (polyvinyl pyrrolidone PVP, added in an amount of 0.3 parts), stir evenly and heat to 120°C, react for 6 hours, evacuate during the reaction, and stir at a high speed of 8000 rpm. After the reaction is completed, dry in a vacuum oven at 100°C for 24 hours to obtain bio-based modified graphene 3#.

[0089] Calculated by mass, 5 parts of bio-based modified graphene 3#, 1 part of sulfur phosphorus alkylphenol zinc salt, 1 part of heavy alkylbenzene sulfonate barium, 40 parts of bio-based base oil, 3 parts of polyisobutylene succinimide and 45 parts of paraffin-based base oil are used to prepare a graphene bio-based anti-wear agent.

[0090] The components and their proportions used in the above examples and comparative examples are shown in Table 1 below:

[0091] Table 1 Example and Comparative Example Group Distribution Ratio

[0092]

[0093]

[0094] Test Example 1

[0095] 1. The graphene bio-based anti-wear agent is added to the commercially available finished oil SL / 10W-40 at a weight ratio of 5%. The four compounded oil samples and the finished oil SL / 10W-40 oil sample were evaluated by a four-ball friction tester to test their anti-friction and anti-wear properties (industry standard SH / TO189-92). Test conditions: GCr15 steel ball, rotation speed 1200r / min, oil temperature 75°C, long grinding time 60min, load 392N. The data given by the four-ball friction tester test include wear spot diameter and friction coefficient. The smaller the wear spot diameter, the higher the anti-wear ability, the smaller the friction coefficient, and the better the friction reduction performance. The results are shown in Table 2 below.

[0096] 2. According to the method of GB / T 5096 petroleum product copper strip corrosion test method, the four compounded oil samples were subjected to copper strip corrosion test, with a corrosion time of 3h and a temperature of 100°C. The results are also shown in Table 2 below.

[0097] Table 2 Test results of various implementation schemes

[0098]

[0099] In addition, the friction curves of some embodiments and comparative examples during the friction test are as follows: Figure 1 As shown, the wear spot test images of the blank finished oil, Example 4 and Comparative Example 2 are shown in sequence. Figure 2a , Figure 2b as well as Figure 2cshown.

[0100] It can be seen from the test results of Table 2 and each figure that, in the finished oil, the wear spot diameter and friction coefficient of the oil sample are reduced by adding the anti-wear agent in Examples 3 and 4, indicating that the graphene bio-based anti-wear agent of the present invention has a good anti-wear and wear-reducing effect; in Comparative Example 1, no graphene is added, the wear spot diameter and friction coefficient increase, and the corrosiveness of the oil sample is enhanced, indicating that graphene can improve the lubrication performance and corrosion resistance of the anti-wear agent; in Comparative Example 2, no bio-based base oil is added, the wear spot diameter and friction coefficient increase, indicating that the bio-based base oil can enhance the lubrication performance of the anti-wear agent and make the lubricating oil have a better anti-wear and wear-reducing effect.

[0101] Test Example 2

[0102] Dispersion stability test, centrifuge accelerated sedimentation (centrifugal force converted to equivalent gravity acceleration multiple)

[0103] Centrifuge at a centrifugal force of 1440 g (1440 times the acceleration of gravity) for 30 minutes (equivalent to natural sedimentation for approximately one month), pause for 30 minutes, and then centrifuge for another 30 minutes. Repeat this process for a total of 4 hours.

[0104] Table 3 Dispersion stability test results

[0105]

[0106] It can be seen from the data in Table 3 that the graphene bio-based anti-wear agent of the present invention can maintain stable dispersion within six months. In fact, due to the centrifugal force that accelerates sedimentation during the deceleration process of the centrifuge, the dispersion stability of the graphene bio-based anti-wear agent can be maintained for more than six months. In the comparative example, since no polyamine substances were added, the number of grafted functional groups was small, and the relative stable dispersion time was shortened to about 3 months. In addition, the use of other functional groups for grafting modification has worse dispersion stability because of poor compatibility with the base oil.

[0107] Through the above control experiments, it can be clearly seen that the key improvement of the present invention compared with many existing technologies is to connect graphene and long fatty chains through polyamine compounds. The role played by the polyamine is multifaceted, not only in significantly improving the grafting rate of the modified group and enhancing the dispersion performance, but also in the change of the affinity between graphene and the metal surface, which brings more excellent anti-wear performance and has important progressive significance.

[0108] In addition, the present invention has also carried out multiple preparation and testing experiments on some other optional polyamine compounds, bio-based fatty acid esters, dispersants, selected additives and other materials, and the same rules were observed, which will not be elaborated here; it can be explained that the main inventive concept of the present invention is based on the physicochemical properties of the graphene composite structure brought about by the high grafting rate generated when the polyamine compounds are connected and applied to the preparation of anti-wear agents; although other factors have a certain influence on the lubrication and dispersion properties, these factors are not essential influencing factors, and equivalent changes to them are all within the core technical concept provided by the present invention.

[0109] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A bio-based modified graphene, characterized in that: The invention comprises graphene, a connecting group and a modifying group connected in sequence, wherein the modifying group comprises a bio-based fatty acid group, the connecting group is derived from a polyamine compound, and different amine groups of the polyamine compound react with epoxy groups and / or carboxyl groups on the surface of graphene oxide to form a connection with the graphene, and react with bio-based fatty acid esters to form a connection with the modifying group.

2. The bio-based modified graphene according to claim 1, characterized in that: The polyamine compound includes any one or a combination of two or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethylenepolyamine, aminoethylpiperazine, polyetheramine, and hydroxyethylethylenediamine; And / or, the bio-based fatty acid ester includes a fatty acid ester formed by a bio-based fatty acid and a lower alcohol; Preferably, the lower alcohol includes any one of methanol, ethanol, propanol, and isopropanol, or a combination of two or more thereof.

3. The method for preparing bio-based modified graphene according to any one of claims 1 to 2, characterized in that: include: Fully mixing graphene oxide, bio-based base oil, and polyamine compound to form a modified reaction system, wherein the bio-based base oil is bio-based fatty acid ester; Different amine groups in the polyamine compound in the modification reaction system are respectively reacted with the epoxy group and / or carboxyl group on the surface of the graphene oxide, and reacted with the bio-based fatty acid ester to form an amide group, so as to obtain bio-based modified graphene.

4. The preparation method according to claim 3, characterized in that: In the modification reaction system, the graphene oxide is 1 part by mass, the bio-based base oil is added in an amount of 10-50 parts by mass, and the polyamine compound is added in an amount of 1-5 parts by mass.

5. The preparation method according to claim 3, characterized in that: The modified reaction system also contains a first dispersant; Preferably, the first dispersant comprises any one or a combination of two or more of polyvinyl pyrrolidone, polymethacrylate, ethylene propylene copolymer, polyisobutylene, and hydrogenated styrene diene copolymer; Preferably, based on 1 part by mass of the graphene oxide, the added amount of the first dispersant is 0.1-0.5 parts by mass.

6. The preparation method according to claim 3, characterized in that: Specifically include: The modified reaction system is heated and emulsified under vacuum conditions, the heating temperature is 80-140° C., the emulsification speed is 8000-14000 rpm, and the reaction time is 4-8 hours; The product obtained after the reaction is completed is dried to obtain the bio-based modified graphene.

7. A graphene bio-based anti-wear agent, characterized in that: The invention comprises a bio-based base oil, a paraffin-based base oil, the bio-based modified graphene according to any one of claims 1 to 2, and a selected auxiliary agent.

8. The graphene bio-based anti-wear agent according to claim 7, characterized in that: The graphene bio-based anti-wear agent comprises 5-10 parts of bio-based modified graphene, 20-40 parts of bio-based base oil, and 40-60 parts of paraffin-based base oil in parts by mass.

9. The graphene bio-based anti-wear agent according to claim 7, characterized in that: The selected additives include antioxidants, rust inhibitors and second dispersants; Preferably, the graphene bio-based anti-wear agent contains 1-3 parts of an antioxidant, 1-3 parts of a rust inhibitor and 3-5 parts of a second dispersant, in parts by mass; Preferably, the antioxidant includes any one of alkylphenol zinc salt, butyl octyl zinc salt, and dioctyl alkaline zinc salt, or a combination of two or more thereof; the rust inhibitor includes any one of heavy alkylbenzene sulfonate barium, petroleum sulfonate barium, alkaline dinonylnaphthalene sulfonate, and dodecenylsuccinic acid, or a combination of two or more thereof; and the second dispersant includes any one of polyisobutylene amine, polyisobutylene succinimide, polyisobutylene succinic anhydride, polyether amine, and Span 80, or a combination of two or more thereof.

10. Use of the graphene bio-based anti-wear agent according to any one of claims 7 to 9 in metal surface lubrication; Preferably, the use comprises use as an engine oil additive.