Rubber tube lubricant and preparation method thereof

By using polyols and thickeners in hose lubricants, combined with metal protective agents, the problem of uneven application caused by hose lubricant residue and high viscosity is solved, achieving good lubrication performance and low residue effects, and is suitable for low-temperature environments. and reduces the risk of contamination.

CN118725950APending Publication Date: 2024-10-01JIANGSU LONGPAN NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410698486.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hose lubricants tend to remain after use, affecting assembly quality and oil purity, and their high viscosity results in uneven application, posing a risk of contamination.

Method used

Polyols are used as lubricating additives, combined with thickeners and metal protective agents, to adjust the viscosity and stability of the lubricant. The homogeneous state and volatility of the lubricant are ensured through the preconditioning of the alkaline base liquid and the addition of the thickener, reducing the Residue.

Benefits of technology

It achieves uniform application of lubricant and good lubrication performance, with very little residue after evaporation, reducing the risk of contamination of the oil. It is suitable for low-temperature environments, and the additives are non-toxic and easy to degrade, and are simple to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a rubber tube lubricant and a preparation method thereof, and the rubber tube lubricant comprises the following components in parts by weight: 80-97 parts of a basic dispersion liquid, 2-6 parts of a thickening agent and 0.1-2 parts of a metal protective agent, the basic dispersion liquid is prepared from 70 to 80 parts of water, 16 to 24 parts of polyhydric alcohol and 1 to 3 parts of organic amine. According to the invention, the polyol is introduced as a lubricating additive, volatilization residues are effectively reduced, the thickening agent is introduced to complement the coating viscosity, the lubricant can fully cover the contact surface of a metal tube and rubber, especially detail parts, during use, the lubricating performance is ensured, the prepared lubricant also can ensure good volatility, after use, the residue is less, and the viscosity is stable. And the lubricant is effectively prevented from influencing other liquid drained through the rubber tube.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a water-based lubricating material, in particular to a hose lubricant, and also to a preparation method of the hose lubricant. Background Art

[0002] During the assembly of a complete vehicle, a large number of hose components are required. These hoses are mainly used in seven systems of oil, gas, drive, control, brake, cooling and heating in the three major parts of the vehicle chassis, engine and body, and play the role of oil supply, gas supply, water supply and power transmission. Hose varieties include fuel pipes, water hoses, brake hoses, vacuum hoses, air conditioning hoses, radiator hoses, power steering hoses and special-shaped branch hoses. The main materials of this type of hose are nitrile rubber, chloroprene rubber and acrylic rubber. At present, wax, lubricating oil or grease are commonly used as lubricants for hose assembly. These three types of lubricants have high viscosity, are not easy to apply evenly, are not easy to volatilize, and some of them remain on the surface after use, resulting in the risk of sliding or loosening of the assembled hose, which may contaminate the surface of the rubber parts. At the same time, there is a risk of entering the vehicle's working oil and contaminating the vehicle's oil, affecting the performance of the vehicle.

[0003] The invention patent application with publication number CN 102311858 A discloses a lubricant for assembling rubber parts and metal parts and a preparation method thereof, comprising: 10 to 60 parts by weight of vegetable oleic acid, 40 to 70 parts by weight of triethanolamine, and 200 to 500 parts by weight of distilled water; the invention patent application with publication number CN 117925310 A discloses a heavy-duty vehicle tire sub-packaging lubricant and a method for sub-packaging lubrication of heavy-duty vehicle tires, the lubricant comprising 0.4 to 0.7% triethanolamine, 0.1 to 0.2% isooctanoic acid, 0.3 to 0.6% oleic acid, 0.15 to 0.25% capric acid, 2.0 to 3.0% polyethylene glycol, and the balance being water. In both schemes, oleic acid and triethanolamine are compounded to adjust the pH value of the solution and generate lubricating and rust-proof triethanolamine oleate at a certain temperature to improve the lubrication effect. After the water content of the lubricant disappears, the lubricating effect is no longer present. In the scheme disclosed in CN102311858A, a large amount of vegetable oleic acid and triethanolamine need to be added to ensure the lubrication effect. In the scheme disclosed in CN 117925310 A, the amount of vegetable oleic acid and triethanolamine added is greatly reduced, but the viscosity of the lubricant is low and needs to be used in conjunction with a spray device. In addition, after the configured lubricant is dried, other additives are likely to remain, affecting the quality of the drainage liquid in the hose. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a hose lubricant that ensures lubrication effect and has little residue; another purpose of the present invention is to provide a method for making a hose lubricant that is simple in making.

[0005] Technical solution: The hose lubricant of the present invention comprises the following components by weight:

[0006] 80 to 97 parts of a basic dispersion, 2 to 6 parts of a thickener, and 0.1 to 2 parts of a metal protective agent; the basic dispersion comprises 70 to 80 parts of water, 16 to 24 parts of a polyol, and 1 to 3 parts of an organic amine.

[0007] In the present invention, polyol is introduced as a lubricating additive to reduce volatile residues, and a thickener is introduced to supplement the coating viscosity. When used, the lubricant can fully cover the contact surfaces of the metal pipe and the rubber, especially the details, to ensure the lubricating performance. After volatilization, there is very little residue on the metal and rubber surfaces, and no residual white spots, which effectively prevents the lubricant from affecting other liquids drained through the hose.

[0008] In the present invention, since more polyols are introduced into the lubricating system, the dispersion system is affected. If the thickener is directly introduced into the mixed system of water and polyols, the thickener cannot exist stably, and flocculation or precipitation is prone to occur during the preparation of the lubricant, which directly affects the product appearance and lubrication effect. Therefore, the basic dispersion needs to be pre-adjusted to alkalinity so that the whole can maintain a homogeneous state after the thickener is added.

[0009] In this case, the introduction of thickeners helps to improve the stability of the lubricant, making it less likely to separate and separate, and the additives less likely to precipitate. The alkaline base fluid also reduces the corrosion of water in the lubricant to the metal.

[0010] Preferably, the lubricant comprises the following components: 90-96 parts of a base dispersion, 3-5 parts of a thickener, and 0.1-1.5 parts of a metal protective agent; the base dispersion comprises 70-80 parts of water, 16-20 parts of a polyol, and 1.4-2 parts of an organic amine.

[0011] Preferably, the polyol is one or more of 1,2-propylene glycol, 1,3-propylene glycol, and 1,4-butylene glycol.

[0012] Preferably, the thickener is one or a mixture of AES-60, hydroxypropyl methylcellulose and hydroxyethyl cellulose.

[0013] Preferably, the lubricant further comprises 0.1 to 0.6 parts of water-soluble polyether ester. The water-soluble polyether ester is used to enhance the lubricating effect of the lubricant. In this solution, the additional introduction of water-soluble polyether ester can also keep the lubricant more volatile, and no white spots will appear after the volatilization.

[0014] Preferably, the organic amine is diglycolamine and / or triethanolamine.

[0015] Preferably, the metal protective agent is one or more of methylbenzotriazole, sebacic acid, and dodecenylsuccinic acid.

[0016] Preferably, the lubricant further comprises 0.01 to 1 part of a bactericide, which is used to prevent the lubricant from deteriorating.

[0017] Preferably, the bactericide is a mixture of one or more of ethylene glycol phenyl ether, kason, polyhexamethylene biguanide hydrochloride and didecyl dimethyl ammonium chloride, wherein ethylene glycol phenyl ether is of reagent grade with a purity greater than 99%, kason has an active ingredient content of ≥1.5%, polyhexamethylene biguanide hydrochloride is of reagent grade with a purity greater than 98%, and didecyl dimethyl ammonium chloride is of reagent grade with a purity greater than 98%.

[0018] The preparation method of a hose lubricant according to the present invention comprises the following steps:

[0019] (1) adding polyol and organic amine into water and stirring until dissolved to obtain a basic dispersion;

[0020] (2) Under vacuum conditions, add a thickener, a metal protective agent, and a bactericide to the basic dispersion, stir, and allow to stand to obtain a hose lubricant.

[0021] Preferably, in step (2), the thickener, metal protective agent and bactericide are added in batches, and each time a reagent is added, a stirring and standing step is performed.

[0022] Preferably, in step (2), the stirring time is 20 to 30 minutes, and the standing time is 50 to 60 minutes.

[0023] Preferably, in step (2), the bactericide is pre-dissolved in the base dispersion or water before being added. Pre-dissolution allows the bactericide to be evenly dispersed in the lubricant system to avoid local deterioration.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) It has both lubricity and volatility: The lubricant prepared can be fully and evenly applied to the surface of rubber parts, has good lubricity, meets the lubrication requirements between parts and rubber, leaves very little residue after volatilization, and does not leave white spots; (2) It is safe, non-toxic and easy to degrade: The additives are all non-toxic, low-toxic, harmless and less harmful, which greatly reduces the harm of lubricants to human body and environment; (3) It is easy to prepare and simple to operate: The lubricant obtained by the present invention has low viscosity, and the preparation is time-saving and labor-saving; (4) It has a wide range of applications: The freezing point of the lubricant of the present invention can reach about -20°C, and it can be used normally even in low temperature conditions in winter; (5) It has good stability: The lubricant prepared is a homogeneous, clear liquid, and the bactericide effectively ensures that the system does not deteriorate, eliminates the need for a defoaming agent, and avoids the uneven material formed by the self-polymerization of the defoaming agent affecting the lubrication effect. DETAILED DESCRIPTION

[0025] The technical scheme of the present invention is further described below. Unless otherwise specified, the reagents used in the following examples are commercially available reagents and are used directly without additional purification. Water-soluble polyether ester was purchased from Notai Biotechnology (Hefei) Co., Ltd.

[0026] Examples 1 to 8: Lubricants were prepared by configuring the components according to the following table:

[0027]

[0028] In the table above, the fungicide is premixed in the proportions in brackets and then added to the lubricant in the proportions outside brackets. The freezing point of the lubricant can be adjusted by adjusting the ratio of water to polyol as required.

[0029] The hose lubricants of Examples 1 to 8 are prepared as follows:

[0030] (1) Add polyol to high-purity water and stir for 20 to 30 minutes until the material is completely dissolved to prepare a lubricant aqueous solution;

[0031] (2) adding the organic amine to the lubricant aqueous solution and stirring for 20 to 30 minutes to obtain a basic dispersion;

[0032] (3) Turn on the negative pressure vacuum pump, add the thickener to the base dispersion at a vacuum degree of -0.095Mpa to -0.1Mpa and a stirring speed of 200 to 300r / min, stir for 20 to 30 minutes, then stop stirring and continue vacuuming for 50 to 60 minutes.

[0033] (4) At a vacuum degree of -0.095 MPa to -0.1 MPa and a stirring speed of 200 to 300 r / min, continue to add the metal protective agent and the fungicide to the basic dispersion respectively, stir for 20 to 30 minutes, then stop stirring and continue vacuuming for 50 to 60 minutes.

[0034] The prepared lubricant was tested for rubber compatibility and metal compatibility according to GB 12981-2012, and the lubricity test was performed using the ramp method. The test results are shown in Table 2.

[0035] Comparative Example 1: Using polymer as lubricating additive

[0036] The lubricant prepared in this comparative example is similar to that in Example 1, except that 1,2-propylene glycol is replaced by PEG-400, and the preparation method is the same as that in Example 1. The lubricating effect of the hose lubricant prepared in this comparative example can meet the actual use requirements, but obvious white spots remain after volatilization.

[0037] Comparative Example 2: Using polyol alone as a lubricant

[0038] This comparative example is similar to Example 1, except that no thickener is added (high-purity water supplements the thickener component). The obtained hose lubricant has a lubricating effect and can basically meet the use requirements, but has poor sagging performance and is not easy to apply.

[0039] Comparative Example 3: Changing the preparation steps

[0040] This comparative example is similar to Example 1, except that, under vacuum conditions, water, polyol, organic amine, thickener, metal protective agent, and bactericide are mixed simultaneously, and the obtained hose lubricant system is unstable and white precipitate appears.

[0041] Comparative Example 4: A certain brand of oil-based automotive hose lubricant on the market, the main lubricating ingredients are: mineral oil, thickener, additives.

[0042] Comparative Example 5: A certain brand of oil-based automotive hose lubricant on the market, the main lubricating ingredients are: mineral oil and additives.

[0043] Comparative Example 6: A certain brand of oil-based automotive hose grease available on the market, the main lubricating ingredients are: mineral oil and additives.

[0044] The automotive hose lubricants of Examples 2 to 5 and Comparative Examples 4 to 6 were tested for metal and rubber compatibility and volatility. The results are shown in the following table.

[0045]

[0046]

[0047] After testing, the automotive hose lubricant provided by the present invention has good compatibility with metal and rubber, and good lubricity. After drying, the lubricants prepared in Examples 1 to 6 have no white spots on the rubber and metal surfaces. In Example 7, the amount of propylene glycol added increased, and the lubricating effect increased, but the volatility experiment showed that the lubricant was not volatile enough, and white spots appeared on the rubber and metal test pieces. In Example 8, the amount of propylene glycol, thickener, etc. added was reduced. After the volatility experiment, sporadic white spots appeared on the rubber and metal test pieces, and the sliding distance of the test piece was less than 10 cm, and the lubricity decreased. During the experiment, the lubricant was unevenly coated.

Claims

1. A hose lubricant, It is characterized in that The invention comprises the following components: by weight, 80 to 97 parts of a basic dispersion liquid, 2 to 6 parts of a thickener, and 0.1 to 2 parts of a metal protective agent; the basic dispersion liquid comprises 70 to 80 parts of water, 16 to 24 parts of a polyol, and 1 to 3 parts of an organic amine.

2. The hose lubricant according to claim 1, It is characterized in that The polyol is one or more of 1,2-propylene glycol, 1,3-propylene glycol, and 1,4-butylene glycol.

3. The hose lubricant according to claim 1, It is characterized in that The thickener is one or a mixture of AES-60, hydroxypropyl methylcellulose and hydroxyethyl cellulose.

4. The hose lubricant according to claim 1, It is characterized in that The lubricant also includes 0.1 to 0.6 parts of water-soluble polyether ester.

5. The hose lubricant according to claim 1, It is characterized in that The organic amine is diglycolamine and / or triethanolamine.

6. The hose lubricant according to claim 1, It is characterized in that The metal protective agent is one or more of methylbenzotriazole, sebacic acid, and dodecenylsuccinic acid.

7. The hose lubricant according to claim 1, It is characterized in that The lubricant also includes 0.01 to 1 part of a bactericide, which is a mixture of one or more of ethylene glycol phenyl ether, kason, polyhexamethylene biguanide hydrochloride and didecyl dimethyl ammonium chloride.

8. A method for preparing the hose lubricant according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) adding polyol and organic amine into water and stirring until dissolved to obtain a basic dispersion; (2) Under vacuum conditions, add a thickener, a metal protective agent, and a bactericide to the basic dispersion, stir, and allow to stand to obtain a hose lubricant.

9. The preparation method according to claim 8, It is characterized in that In the step (2), the thickener, metal protective agent and bactericide are added in batches, and each time a reagent is added, a stirring and standing step is performed.

10. The preparation method according to claim 9, It is characterized in that In the step (2), the stirring duration is 20 to 30 minutes, and the standing duration is 50 to 60 minutes.

Citation Information

Patent Citations

  • Lubricant for assembling rubber articles and metal parts, and manufacturing method thereof

    CN102311858A

  • Heavy-duty car tire split charging lubricating agent and heavy-duty car tire split charging lubricating method

    CN117925310A