Method for improving sulfides in steel by accurately blowing magnesium oxide nanoparticles
By using MgO nanoparticle injection technology in the steelmaking process, the injection amount of MgO nanoparticles is dynamically adjusted according to the S content in the molten steel, which solves the problem of controlling the morphology and distribution of sulfides in steel, improves the mechanical properties of the steel, and reduces the Production costs and risk of water outlet clogging.
Patent Information
- Application Number
- CN202410749426.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to accurately control the morphology and distribution of sulfides in steel with existing steelmaking technology, resulting in a decrease in the mechanical properties of the steel. Moreover, the method of feeding magnesium-calcium alloy wire is costly and cumbersome, and the magnesium yield is unstable, which can easily lead to nozzle blockage and Cleanliness decreases.
Using MgO nanoparticle injection technology, MgO nanoparticles are added through bottom blowing after RH vacuum refining. The injection amount of MgO nanoparticles is dynamically adjusted according to the S content in the molten steel to form an effective nucleation core and improve the size of sulfides. shape and distribution to avoid external impurities such as Al, Si, and Ca.
It achieves effective modification of MnS inclusions, reduces the proportion of long strips of MnS, improves the mechanical properties of steel, reduces the risk of nozzle blockage, and ensures the purity of molten steel and the production environment.
Smart Images

Figure CN118726700A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steelmaking, and in particular relates to a method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles. Background Art
[0002] Sulfur usually has a harmful effect on most steel grades, but in recent years, many steels often require higher sulfur content due to their special performance requirements, such as controlling sulfur in heavy rail steel at 0.009% to 0.015% to resist hydrogen-induced fracture, and S content in wheel steel at 0.008% to 0.02% to improve cutting performance. In steel, sulfides mainly exist in the form of MnS. The uniformly distributed MnS inclusions in steel are an important guarantee for the good cutting performance of steel. However, with the gradual increase in sulfur content in high-speed rails, heavy-load rails and other steels, the unqualified rating rate of MnS inclusions in steel has increased significantly. The long strip MnS inclusions that undergo severe deformation after rolling lead to reduced mechanical and fatigue properties of steel, hindering the development of high-grade steel. Therefore, one of the important directions for the development of domestic steel at present is to reduce long strip MnS inclusions and form spherical inclusions such as "MnS wrapped oxides".
[0003] Magnesium oxide particles have a good modification effect on alumina and manganese sulfide in steel, but due to the physical and chemical properties of magnesium metal, there are problems such as violent reaction, unstable yield, and difficulty in accurately controlling the magnesium content and inclusions in steel after adding to molten steel. The added magnesium oxide particles are thermally stable and hardly decompose. On the one hand, after MgO nanoparticles are sprayed into the molten steel, [Al] and [O] in the steel diffuse into the MgO core to form MgAl2O4, or [Al] and [O] react to form Al2O3 and then form MgAl2O4 through the collision reaction of particles, which can achieve the modification of alumina inclusions in steel; on the other hand, the stable MgO particles and the MgAl2O4 generated by the reaction can serve as the effective nucleation core for the precipitation of manganese sulfide inclusions, transforming the long strip pure MnS into spherical and spindle-shaped composite inclusions with oxide as the core, improving the sulfide morphology and reducing the rolling deformation of sulfide.
[0004] CN110656280A "Low-oxygen calcium-magnesium-sulfur free-cutting steel and its preparation method" adopts the method of feeding magnesium wire into the molten steel first and then calcium wire, or feeding magnesium-calcium wire to carry out magnesium-calcium composite treatment on the molten steel. This method can control the morphology of sulfide inclusions in the steel and improve the mechanical properties of the steel, but the steelmaking cost increases, the process is relatively cumbersome, and it is difficult to accurately control the content of Ca and Mg fed into the steel, which is prone to large-sized inclusions and nozzle blockage problems.
[0005] CN107312907A "A method for controlling the morphology of manganese sulfide in medium-low sulfur and low oxygen steel" uses a wire feeder to feed calcium-magnesium alloy wire into the molten steel after aluminum deoxidation. This method denatures the pure MnS inclusions in the steel into composite sulfides (Ca, Mn)S, (Mg, Mn)S and (Ca, Mg, Mn)S, which are rolled into spindle-shaped composite sulfides. This invention patent is only applicable to medium-low sulfur and low oxygen steel, and the magnesium yield is low and the magnesium content is difficult to achieve precise control.
[0006] CN111304407A "A method for treating molten steel with magnesium and calcium by spraying powder at a long nozzle" uses a long nozzle to spray fine magnesium powder or calcium powder to treat molten steel with magnesium and calcium during the molten steel casting process, thereby improving the recovery rate of magnesium and calcium. However, the uniformity of the magnesium powder sprayed at the long nozzle of the invention is poor, and the modification effect and particle size improvement of MnS inclusions after spraying magnesium powder are not reflected, and the influence of spraying magnesium powder on the nucleation of inclusions is not studied.
[0007] CN112063916A "Preparation method of magnesium-based high-sulfur free-cutting steel" feeds magnesium-containing cored wire into the molten steel to modify the inclusions in the steel, and the proportion of composite inclusions is significantly increased. However, the fed magnesium-containing cored wire contains a large amount of Si, Al or Ca elements in addition to magnesium, and a large amount of SiO2, Al2O3, and CaO inclusions will be introduced into the molten steel after the cored wire is fed. Especially for high-sulfur and high-oxygen steel, in actual production, there is almost no pure MgO inclusion after the cored wire is fed, and a large amount of MgO·Al2O3 inclusions are generated by reaction, which easily leads to problems such as nozzle blockage and reduced cleanliness. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a method for accurately spraying magnesium oxide nanoparticles to improve sulfides in steel. By establishing a dynamic adjustment model for MgO spraying, MgO nanoparticles are added by bottom blowing after RH vacuum refining, and the MgO spraying amount is dynamically adjusted according to the S content of the molten steel. Under the premise of not introducing impurity elements such as Al, Si, Ca into the molten steel from the outside, an effective nucleation core is provided for the precipitation of MnS in the steel, and the size, morphology and distribution of sulfides in the steel are accurately improved.
[0009] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0010] A method for accurately spraying magnesium oxide nanoparticles to improve sulfides in steel includes converter or electric furnace smelting, LF refining outside the furnace, RH vacuum refining, and continuous casting. In the RH vacuum refining step, MgO nanoparticles are added by bottom blowing after vacuum refining. The relationship between the amount of MgO nanoparticles added and the S content in the molten steel is:
[0011] Y=5.01-4.56 / [1+(X / 0.21) 2.45], and 0.01≤X≤0.5, 0.45≤Y≤4.52;
[0012] R 2 =0.985;
[0013] Where:
[0014] Y——the amount of MgO nanoparticles added, kg;
[0015] X——mass content of S in molten steel, %;
[0016] R 2 ——Regression coefficient, the closer it is to 1, the more accurate the prediction of the formula is.
[0017] Furthermore, the particle size of the MgO nanoparticles is 20 to 50 nm, and the purity is above 99.9%.
[0018] Furthermore, in the RH vacuum refining step, the RH vacuum treatment pressure is 65-75 Pa, and the vacuum treatment time is ≥20 min.
[0019] Furthermore, in the RH vacuum refining process, MgO nanoparticles are added by bottom blowing and then soft blowing is performed for 5 to 15 minutes.
[0020] Furthermore, the steel components and their mass percentages are: C: 0.20-0.60%, Si: 0.15-0.65%, Mn: 0.60-1.50%, P≤0.020%, S: 0.01-0.50%, Cr: 0.15-0.65%, Al: 0.010-0.050%, Ca: 0.0005-0.002%, Mg≤0.002%, and the remainder is Fe and unavoidable impurities.
[0021] The beneficial effects of adopting the above technical solution are:
[0022] 1. Based on the basic principles of thermodynamics and kinetics and the actual smelting conditions, a dynamic adjustment model for MgO nanoparticle injection was established to achieve accurate and dynamic adjustment of the MgO nanoparticle injection amount under different S contents, avoiding the problem of unstable magnesium content caused by wire feeding and decreased cleanliness of molten steel caused by excessive magnesium content.
[0023] 2. Without introducing impurity elements such as Al, Si, and Ca into the molten steel from the outside, MgO nanoparticles are directly used for sulfide modification, which reduces the large-sized Al2O3, SiO2 and other oxide inclusions brought into the steel by the magnesium alloy wire, improves the blockage of the continuous casting nozzle, and has significant social and economic benefits.
[0024] 3. There is no oxidation chemical reaction of Mg, and the nucleation core is not generated by oxidation reaction. There are no problems such as violent reaction and splashing caused by wire feeding, which ensures the purity of molten steel and a good production environment.
[0025] 4. RH refining bottom blowing MgO nanoparticles, MgO nanoparticles are evenly dispersed in the molten steel, fully modifying the MnS inclusions in the steel, increasing the proportion of MnS composite inclusions from 4.7% to more than 15%, and reducing the proportion of sulfide aspect ratio ≥3 in the rolled product from 52% to less than 33%. The fine series of Class A inclusions are ≤1.5 level, and the coarse series are ≤0.5 level. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is the relationship between the injection amount of MgO nanoparticles and the S content in the steel of the present invention;
[0027] Figure 2 , 3 The typical (Al2O3·MgO)-MnS inclusion morphology and composition diagram in the steel after the injection of MgO nanoparticles in the present invention;
[0028] Figure 4 The ratio of sulfide composite inclusions in the steel obtained in Examples 1-5;
[0029] Figure 5 The proportion of sulfides with an aspect ratio ≥ 3 in the steel obtained in Examples 1-5;
[0030] Figure 6 The test results of fine and coarse type A inclusions in steel obtained in Examples 1-5;
[0031] Figure 7 The statistical results of the average size of inclusions in steel obtained in Examples 1-5 are shown. DETAILED DESCRIPTION
[0032] Example 1
[0033] (1) RH vacuum refining process: RH vacuum refining time is 20 min, vacuum degree is 65 Pa, after refining, MgO nanoparticles are added in bottom blowing, soft blowing is performed for 5 min, and the mixture is allowed to stand for 10 min.
[0034] (2) The weight of the molten steel is 130 tons, the sulfur content is 0.010%, and the particle size of the sprayed MgO nanoparticles is 20 nm. According to the relationship between the amount of MgO nanoparticles added Y and the sulfur content X in the molten steel: Y = 5.01-4.56 / [1+(X / 0.21) 2.45 ] calculated, the injection amount of MgO nanoparticles is 0.45kg.
[0035] Example 2
[0036] (1) RH vacuum refining process: RH vacuum refining time is 28 min, vacuum degree is 65 Pa, after refining, MgO nanoparticles are added by bottom blowing, soft blowing is performed for 10 min, and the mixture is allowed to stand for 10 min.
[0037] (2) The weight of the molten steel is 130 tons, the sulfur content is 0.28%, and the particle size of the sprayed MgO nanoparticles is 25 nm. According to the relationship between the amount of MgO nanoparticles added Y and the sulfur content X in the molten steel: Y = 5.01-4.56 / [1+(X / 0.21) 2.45 ] calculated, the injection amount of MgO nanoparticles is 3.5kg.
[0038] Example 3
[0039] (1) RH vacuum refining process: RH vacuum refining time is 32 min, vacuum degree is 70 Pa, after refining, MgO nanoparticles are added in bottom blowing, soft blowing is performed for 10 min, and the mixture is allowed to stand for 10 min.
[0040] (2) The weight of the molten steel is 130 tons, the sulfur content is 0.37%, and the particle size of the sprayed MgO nanoparticles is 29 nm. According to the relationship between the amount of MgO nanoparticles added Y and the sulfur content X in the molten steel: Y = 5.01-4.56 / [1+(X / 0.21) 2.45 ] calculated, the injection amount of MgO nanoparticles is 4.10kg.
[0041] Example 4
[0042] (1) RH vacuum refining process: RH vacuum refining time is 29 minutes, vacuum degree is 75 Pa, after refining, MgO nanoparticles are added by bottom blowing, soft blowing is performed for 15 minutes, and the mixture is allowed to stand for 10 minutes.
[0043] (2) The weight of the molten steel is 130 tons, the sulfur content is 0.15%, and the particle size of the sprayed MgO nanoparticles is 42 nm. According to the relationship between the amount of MgO nanoparticles added Y and the sulfur content X in the molten steel: Y = 5.01-4.56 / [1+(X / 0.21) 2.45 ] calculated, the injection amount of MgO nanoparticles is 1.84kg.
[0044] Example 5
[0045] (1) RH vacuum refining process: RH vacuum refining time is 27 min, vacuum degree is 75 Pa, after refining, MgO nanoparticles are added in bottom blowing, soft blowing is performed for 15 min, and the mixture is allowed to stand for 10 min.
[0046] (2) The weight of the molten steel is 130 tons, the sulfur content is 0.50%, and the particle size of the sprayed MgO nanoparticles is 50 nm. According to the relationship between the amount of MgO nanoparticles added Y and the sulfur content X in the molten steel: Y = 5.01-4.56 / [1+(X / 0.21)2.45 ] calculated, the injection amount of MgO nanoparticles is 4.52kg.
[0047] The composition and mass content of the finished molten steel of Examples 1-5 are shown in Table 1; the detection results of inclusions in the steel are shown in Table 2.
[0048] Table 1. Composition and mass content of finished molten steel of Examples 1-5 (%)
[0049] Example C Si Mn P S Cr Al Ca Mg 1 0.20 0.15 0.60 0.020 0.01 0.27 0.010 0.0005 0.0002 2 0.32 0.46 1.08 0.015 0.28 0.15 0.028 0.0019 0.0016 3 0.44 0.27 1.20 0.017 0.37 0.35 0.030 0.0010 0.0019 4 0.47 0.37 1.32 0.014 0.15 0.47 0.033 0.0020 0.0008 5 0.60 0.65 1.50 0.016 0.50 0.65 0.050 0.0012 0.0020
[0050] In Table 1, the balance is Fe and unavoidable impurities.
[0051] Table 2. Inclusion detection results of Examples 1-5
[0052]
[0053] The morphology of the steel sulfide inclusions produced in Examples 1-5 is well controlled, and the inclusion detection results are shown in Table 2 and Appendix. Figure 1-7 As shown in the figure, a large number of complex sulfides are generated in the steel, with fewer thin strip sulfides. The proportion of sulfide composite inclusions increases from 4.7% to more than 15%, and the proportion of sulfide aspect ratio ≥ 3 in the rolled product decreases from 52% to less than 33%. The fine series of Class A inclusions is ≤1.5 level, the coarse series is ≤0.5 level, and the average size of inclusions is controlled between 1-3μm.
[0054] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles, comprising converter or electric furnace smelting, LF refining, RH vacuum refining, and continuous casting steps, characterized in that: In the RH vacuum refining process, MgO nanoparticles are added by bottom blowing after vacuum refining. The relationship between the amount of MgO nanoparticles added and the S content in the molten steel is: Y=5.01-4.56 / [1+(X / 0.21) 2.45 ], and 0.01≤X≤0.5, 0.45≤Y≤4.52; R 2 =0.985; Where: Y——the amount of MgO nanoparticles added, kg; X——mass content of S in molten steel, %; R 2 ——Regression coefficient, the closer it is to 1, the more accurate the prediction of the formula is.
2. The method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles according to claim 1, characterized in that: The particle size of the MgO nanoparticles is 20-50 nm, and the purity is above 99.9%.
3. The method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles according to claim 2, characterized in that: In the RH vacuum refining process, the RH vacuum treatment pressure is 65-75 Pa, and the vacuum treatment time is ≥20 min.
4. The method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles according to claim 3, characterized in that: In the RH vacuum refining process, MgO nanoparticles are added by bottom blowing and then soft blowing is performed for 5 to 15 minutes.
5. The method for improving sulfides in steel by precisely spraying magnesium oxide nanoparticles according to any one of claims 1 to 4, characterized in that: The steel components and their mass percentages are: C: 0.20-0.60%, Si: 0.15-0.65%, Mn: 0.60-1.50%, P≤0.020%, S: 0.01-0.50%, Cr: 0.15-0.65%, Al: 0.010-0.050%, Ca: 0.0005-0.002%, Mg≤0.002%, and the remainder is Fe and unavoidable impurities.
Citation Information
Patent Citations
Method for smelting steel for large heat input welding pipeline
CN101591719A
Optimized method for removing sulfur from magnesium granules
CN102382942A
Method for refining grain size of sulfur-containing non-quenched and tempered steel
CN112195305A
Corrosion-resistant and fire-resistant steel with excellent high-temperature creep property under uniaxial tension and production method of corrosion-resistant and fire-resistant steel
CN114875329A
Low-carbon low-sulfur steel magnesium treatment process
CN114908218A