Method for reducing iron loss of oriented silicon steel through online laser nicking

By regulating the groove depth, spacing and scanning speed of laser marking, the problem of improving the uniformity of steel plate iron loss under different thicknesses and operating speeds is solved, achieving efficient iron loss reduction and maintaining production efficiency.

CN118726718APending Publication Date: 2024-10-01GUANGZHOU SUNINE INTELLIGENT TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410769644.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology cannot effectively solve the problem of improving the uniformity of iron loss of steel plates under different thicknesses and operating speeds in reducing the iron loss of grain-oriented silicon steel, and affects production efficiency.

Method used

By regulating the groove depth, spacing and scanning speed of the laser notch, coordinated regulation is carried out according to the steel plate thickness and operating speed to ensure the iron loss improvement effect of the steel plate under different thicknesses and speeds, and to avoid damage and dislocation of the insulating coating caused by the notch. Caused by increased iron losses.

Benefits of technology

The iron loss improvement rate of steel plates under different thicknesses and different operating speeds is achieved to reach more than 15%, maintaining high production efficiency and avoiding the offset of the iron loss reduction effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004893719920000051
    Figure BDA0004893719920000051
  • Figure BDA0004893719920000052
    Figure BDA0004893719920000052
  • Figure BDA0004893719920000061
    Figure BDA0004893719920000061
Patent Text Reader

Abstract

The invention belongs to the field of oriented silicon steel manufacturing, and particularly discloses a method for reducing steel loss of oriented silicon steel through online laser nicking. According to the method, the laser scanning speed, the indentation groove width and the groove depth are regulated and controlled by pertinently combining the steel belt running speed and the steel belt thickness, and on the basis of coordinated regulation and control of the laser scanning speed, the indentation groove width and the groove depth, online laser indentation is carried out on the stretched and flattened annealed wire; the method has an excellent steel plate iron loss improvement effect on steel strips with different thicknesses and running at different steel strip speeds, and the production efficiency of oriented silicon steel is not affected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of grain-oriented silicon steel manufacturing, and specifically relates to a method for reducing wear and tear on grain-oriented silicon steel through online laser marking. Background Technology

[0002] Grain-oriented silicon steel is a fundamental material used in the manufacture of transformer equipment. Transformers consume a large amount of electrical energy due to iron losses, therefore, reducing iron losses is a relentless goal in the production of grain-oriented silicon steel. Iron losses in silicon steel sheets can be divided into hysteresis losses and eddy current losses. Eddy current losses can be further divided into classical eddy current losses (caused by eddy currents) and anomalous eddy current losses (caused by magnetic wall motion, proportional to the magnetic domain width). Under power frequency conditions, anomalous eddy current losses account for about half of the iron losses. Therefore, many steel companies and research institutes at home and abroad have conducted research on magnetic domain refinement technology, and have successively developed surface treatment technologies such as machining, laser irradiation, electrical discharge treatment, plasma flow irradiation, local heating, ultrasonic vibration, and jet fluid methods. These technologies refine the magnetic domains by reducing the 180° magnetic domain wall spacing, thereby achieving the goal of reducing iron losses. Among these, laser marking is the most prominent method.

[0003] Laser irradiation utilizes the heat of a laser beam to create an elastic-plastic deformation zone beneath the surface of a steel plate. The compressive stress generated in this zone and the tensile stress between the indentations reduce the width of the main domains in the grain-oriented silicon steel, thereby lowering its eddy current losses. This method significantly reduces iron loss and, being a non-contact process, offers very high reliability and controllability.

[0004] Patent CN102477484A proposes a rapid laser marking method that simultaneously performs laser marking on the upper and lower surfaces of grain-oriented silicon steel strip. A highly focused continuous-wave laser beam is used to simultaneously mark lines on both surfaces of the running strip. The marking lines on the upper and lower surfaces are arranged in an equally spaced, intersecting pattern to ensure uniform improvement in iron loss. The spacing between marking lines on a single surface of the strip is 6-12 mm, the laser power is 1000-3000W, and the scanning speed is 100-400 m / min. This method achieves a processing speed 1.5-2 times that of traditional single-sided laser marking methods. However, this method requires simultaneous laser marking on both the upper and lower surfaces of the strip. While this method improves the production efficiency of grain-oriented silicon steel, it does not consider the issue of uniformity in iron loss improvement for steel strips of different thicknesses and running speeds.

[0005] Patent CN116475581A proposes a laser marking method for unequal power partitions of grain-oriented silicon steel. The method divides the grain-oriented silicon steel strip into three transverse partitions, with each partition corresponding to a laser head. The three laser heads are arranged at the same height, and each head uses a different power to simultaneously laser-mark the surface of the corresponding transverse partition of the grain-oriented silicon steel strip. This invention addresses the uneven distribution of performance and surface condition in the transverse direction of grain-oriented silicon steel coils by dividing the entire coil into transverse partitions and using a process scheme with different power levels for laser marking of different partitions. While ensuring a significant reduction in loss through marking across the entire coil of grain-oriented silicon steel strip, it avoids or minimizes damage to the insulating coating, thereby obtaining grain-oriented silicon steel products with excellent magnetic properties and surface quality. However, this laser marking process must be performed after the grain-oriented silicon steel leveling, stretching, and annealing line (CT line). The power for laser marking must be selected based on the quality inspection table and the online iron loss curve results of the CT line, significantly reducing production efficiency. Furthermore, it does not consider the issue of improving the uniformity of iron loss improvement in steel plates under different thicknesses and running speeds of steel strips.

[0006] Patent CN111571024A discloses an application of a laser marking machine for dynamic synchronous marking on a stretching and leveling annealing unit. The laser marking machine is located between the tension machine and the magnetometer in a CT production line. Multiple laser heads of the laser marking machine alternately mark to ensure synchronous dynamic marking of the grain-oriented silicon steel strip. The marking width is controlled by adjusting the height of the multiple laser heads, the marking depth is controlled by adjusting the focal length of the multiple laser heads, and the corresponding time of the multiple laser heads is controlled to meet the marking interval requirements. While this method improves the production efficiency of grain-oriented silicon steel and realizes the online application of laser marking in the stretching and leveling process, it does not consider the issue of improving the uniformity of iron loss in the steel plate under different thicknesses and running speeds of steel strips. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing technologies by providing a method for reducing steel loss in grain-oriented silicon steel through online laser marking. This method involves specifically designing and controlling the laser scanning speed, marking groove width, and groove depth in conjunction with the steel strip running speed and thickness. Based on their synergistic control, it achieves excellent steel loss reduction effects under different steel strip thicknesses and running speeds, without affecting the production efficiency of grain-oriented silicon steel.

[0008] To achieve the above-mentioned objectives, the technical solution adopted by the present invention is as follows:

[0009] A method for reducing steel loss in grain-oriented silicon steel using online laser marking involves performing online laser marking on a stretching and flattening annealing line. The depth 'a' of the laser-marked groove is related to the steel plate thickness 'h' by the following formula:

[0010] h × 10% ≤ a ≤ h × 15% (1)

[0011] In the formula, h is the thickness of the steel plate, in mm; a is the depth of the notch groove, in mm;

[0012] The thinner the steel plate, the finer its magnetic domains. Compared with conventional thick steel plates (0.27-0.30mm), thin steel plates (0.18-0.23mm) have smaller magnetic domain widths. The effect of refining magnetic domains through scoring is not significant, and the effect of scoring in further reducing iron loss is also weak, generally less than 10%. According to the relation (1) of the present invention, adjusting the groove depth for different steel strip thicknesses can achieve excellent magnetic domain refinement and iron loss improvement for steel strips of different thicknesses by coordinating the scoring spacing and laser scanning speed. This avoids the problem that excessively deep scoring grooves can damage the insulating coating on the surface of the steel plate, reduce the insulation of the steel plate, and may also cause the effect of increasing iron loss caused by dislocations in the grain structure to cancel out the effect of refining magnetic domains, affecting the reduction of iron loss. It also avoids the problem that excessively shallow scoring grooves cannot effectively reduce the iron loss of the steel strip.

[0013] The spacing b between two adjacent notches is related to the thickness h of the steel plate by the following formula:

[0014] e 5×h ≤ b ≤ e 7×h (2)

[0015] In the formula, h is the thickness of the steel plate, in mm; b is the scribing spacing, in mm;

[0016] The groove depth and groove spacing together affect the refinement of magnetic domains and further improvement of iron loss. According to the relationship (2) of the present invention, the groove spacing can be adjusted for different steel strip thicknesses. Based on the coordinated control of groove depth, groove spacing and laser scanning speed, the goal of excellent magnetic domain refinement and iron loss improvement of steel strips of different thicknesses can be achieved. If the groove spacing is too wide, the goal of effectively reducing iron loss cannot be achieved. If the groove spacing is not too narrow, the laser-etched area will partially overlap, resulting in excessive internal stress in the repeated action area, generating more dislocations, affecting the grain orientation, and causing the iron loss reduction effect of silicon steel to be insignificant.

[0017] The scanning speed C of laser marking is related to the groove depth a, the marking spacing b, and the steel strip speed V by the following formula:

[0018] C = 1.2 × b / a + 0.06 × V (3)

[0019] In the formula, a is the groove depth (mm); b is the groove spacing between two adjacent grooves (mm); V is the running speed of the steel strip (mm / s); and C is the scanning speed of the laser marking (mm / s).

[0020] The running speed V of the steel strip is 1000-3000 mm / s, and the scanning speed C of the laser marking is in mm / s.

[0021] As the thickness of the steel strip varies, the production speed of the steel strip on site will also be adjusted. Different steel strip thicknesses will result in different on-site running speeds, and the same laser marking scanning speed will produce different marking effects due to different on-site steel strip running speeds. Based on the relationship (3) of this invention, the laser scanning speed is controlled by combining the on-site running speed of the steel strip with the groove depth and marking spacing. Based on the coordinated control of the steel strip running speed, the groove depth and marking spacing, the purpose of reducing the iron loss of oriented silicon steel by laser marking at different steel strip thicknesses and running speeds can be achieved. This is beneficial to achieving an iron loss improvement rate of more than 15% for oriented silicon steel at different thicknesses and running speeds. The laser scanning speed of laser marking should not be too fast. Too fast a speed will shorten the time the laser acts on the silicon steel surface, and the internal stress and thermal effect generated by the laser on the silicon steel surface will be smaller, resulting in insufficient refinement of magnetic domains and a worse iron loss reduction effect. The laser scanning speed should not be too slow. If it is too slow, the internal stress and thermal effect generated by the laser on the silicon steel surface will be too large. This may cause the effect of increasing iron loss caused by dislocations in the grain structure to cancel out the effect of refining magnetic domains, thus affecting the improvement of iron loss.

[0022] Therefore, based on the relationship (1) for controlling the groove depth, the relationship (2) for controlling the spacing between adjacent grooves, and the relationship (3) for controlling the laser scanning speed, this invention realizes the control of the groove depth for steel strips of different thicknesses and further controls the spacing between two adjacent grooves for steel strips of different thicknesses. Based on the coordinated control of groove depth, groove spacing and laser scanning speed, the iron loss improvement rate of steel strips of different thicknesses and different running speeds reaches more than 15%.

[0023] In this invention, the thickness of the applicable steel strip is 0.18-0.30 mm.

[0024] In this invention, the applicable steel composition and weight percentage content are as follows: C: 0.04%-0.08%, Si: 3.0%-3.4%, Mn: 0.06%-0.12%, S: 0.01%-0.03%, Als: 0.02%-0.03%, N: 0.006%-0.01%, with the balance being Fe and unavoidable impurities.

[0025] In this invention, molten steel is smelted in a converter and continuously cast. The billet is heated to 1100-1250°C, then conventionally hot rolled, normalized annealed, and then cold rolled to a finished thickness of 0.18-0.30 mm. It then undergoes decarburization annealing, nitriding annealing, coating with magnesium oxide annealing release agent, high-temperature annealing, and after exiting the furnace, it goes to the stretching and leveling process, where an insulating coating is applied, leveling stretching annealing is performed, and laser scoring is applied.

[0026] According to the above scheme, the laser marking equipment is set after the steel plate comes out of the flattening and stretching annealing furnace and before the online iron loss measuring instrument. After the steel plate is laser-marked, it is rolled into finished grain-oriented silicon steel coils.

[0027] The beneficial effects of this invention are:

[0028] The traditional manufacturing process for low-temperature, high-magnetic-induction oriented silicon steel includes: steelmaking, hot rolling, pickling and normalizing, cold rolling, decarburization annealing, nitriding, coating with magnesium oxide release agent, high-temperature annealing, coating with insulating coating, leveling and stretching annealing, laser marking, and finishing. After the leveling and stretching annealing process, the finished oriented silicon steel is transferred to the laser marking unit. However, the slow strip speed affects the production efficiency of low-iron-loss oriented silicon steel and fails to address the stability issue of improving iron loss in steel plates of different thicknesses and at different strip speeds.

[0029] The online laser marking method provided by this invention, through targeted design and control of the scanning speed, marking groove width, and groove depth in conjunction with the steel plate running speed and steel strip thickness, achieves excellent steel plate iron loss improvement under different steel strip thicknesses and running speeds at speeds ranging from 1000 mm / s to 3000 mm / s. Under different steel strip thicknesses and running speeds, the iron loss improvement rate of the steel plate before and after marking can reach 15%, achieving excellent steel plate iron loss improvement effects under different steel strip thicknesses and running speeds without affecting the production efficiency of grain-oriented silicon steel. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0031] Each embodiment of the present invention is prepared according to the following steps:

[0032] 1) Molten steel is smelted in a converter and continuously cast, the billet is heated to 1100-1250℃, and then conventionally hot rolled;

[0033] 2) Normalizing and annealing, then cold rolling to a finished thickness of 0.18-0.30 mm;

[0034] 3) Perform decarburization and nitriding annealing, and apply magnesium oxide annealing release agent;

[0035] 4) High-temperature annealing;

[0036] 5) Apply insulating coating, stretch and smooth annealing, and laser scoring.

[0037] The process parameters for laser marking are as described in Table 1, and the iron loss of the steel plate before and after marking is shown in Table 2.

[0038] In this invention, the preferred composition and weight percentage of the steel used are: C: 0.04%-0.08%, Si: 3.0%-3.4%, Mn: 0.06%-0.12%, S: 0.01%-0.03%, Als: 0.02%-0.03%, N: 0.006%-0.01%, with the balance being Fe and unavoidable impurities. Specifically, in one embodiment, the steel used in this invention has the following composition: C: 0.04%, Si: 3.0%, Mn: 0.06%, S: 0.01%, Als: 0.02%, N: 0.006%, with the balance being Fe and unavoidable impurities. Table 1 shows the process parameters for laser etching in Examples 1-8 and Comparative Examples 1-2. Example 1

[0039]

[0040] The steel composition and weight percentage content are as follows: C: 0.04%, Si: 3.0%, Mn: 0.06%, S: 0.01%, Als: 0.02%, N: 0.006%, with the balance being Fe and unavoidable impurities.

[0041] Molten steel is smelted in a converter and continuously cast. The billet is heated to 1100–1250℃ and conventionally hot-rolled; normalizing annealing is performed, followed by cold rolling to a finished thickness of 0.20 mm; decarburization and nitriding annealing are then performed, followed by coating with a magnesium oxide annealing release agent; high-temperature annealing; coating with an insulating liquid; stretching and leveling annealing; and laser scoring. The laser scoring parameters are shown in Table 1. Magnetic measurements were performed on the steel plates before and after scoring, and the magnetic properties of the steel plates are shown in Table 2.

[0042] Table 2. Magnetic properties of the grain-oriented silicon steel scored products obtained in Examples 1-8 and Comparative Examples 1-2

[0043]

[0044]

[0045] The above experimental results show that:

[0046] In Examples 1-8, when the laser marking process parameters all meet the process range of the technical solution of the present invention, the iron loss improvement rate of the steel plate before and after marking reaches more than 15%, and a low-temperature high magnetic induction oriented silicon steel marking product with low iron loss can be obtained.

[0047] In Comparative Example 1, when the groove depth a does not satisfy the relationship (1) proposed in this invention and the laser marking scanning speed C does not satisfy the relationship (3) proposed in this invention, the steel plate iron loss improvement rate is 1.11%. When the groove depth is too deep and the laser marking scanning speed is too slow, the effect of increasing iron loss caused by dislocations in the grain structure is offset by the effect of refining magnetic domains, resulting in a smaller reduction in iron loss.

[0048] In Comparative Example 2, when the groove depth a does not satisfy the relationship (1) proposed in this invention, the groove spacing b does not satisfy the relationship (2) proposed in this invention, and the laser marking scanning speed C does not satisfy the relationship (3) proposed in this invention, the steel plate iron loss improvement rate is 1.22%. When the groove depth a is too shallow, the groove spacing is too narrow, and the laser marking scanning speed is too fast, the laser marking influence area will partially overlap, the internal stress in the repeated action area will be too large, and more dislocations will be generated, affecting the grain orientation, thus making the effect of laser marking in reducing silicon steel iron loss insignificant.

[0049] The above results collectively demonstrate that the groove depth *a*, groove spacing *b*, and laser marking scanning speed *C* jointly affect the iron loss improvement effect of this invention. This invention, through targeted design and control of the scanning speed, groove width, and groove depth in conjunction with the steel plate running speed and steel strip thickness, achieves excellent iron loss improvement for steel plates at running speeds of 1000 mm / s to 3000 mm / s under different steel strip thicknesses and speeds, without affecting the production efficiency of grain-oriented silicon steel. Furthermore, it achieves excellent iron loss improvement for steel plates under different steel strip thicknesses and speeds. Under different steel strip thicknesses and speeds, the iron loss improvement rate of steel plates after online marking using the method of this invention can reach 15%.

[0050] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A method for reducing steel loss of oriented silicon steel by online laser scoring, characterized in that: On-line laser scoring is performed on the stretching flattening annealing line. The depth a of the scoring groove in the laser scoring and the thickness h of the steel plate have the following relationship: h × 10% ≤ a ≤ h × 15% (1) Where, h is the thickness of the steel plate, in mm; a is the depth of the notch groove, in mm; The notch spacing b between two adjacent notches and the steel plate thickness h have the following relationship: e 5×h ≤ b ≤ e 7×h (2) Where, h is the thickness of the steel plate, in mm; b is the notch spacing, in mm; The scanning speed C of laser scoring has the following relationship with the scoring groove depth a, scoring spacing b, and steel belt speed V: C = 1.2×b / a+0.06×V (3) Where a is the groove depth, in mm; b is the spacing between two adjacent notches, in mm; V is the running speed of the steel strip, in mm / s; C is the scanning speed of the laser notch, in mm / s. The running speed V of the steel belt is 1000-3000 mm / s, and the scanning speed C of the laser scoring is in units of mm / s.

2. The method according to claim 1, characterized in that: The thickness of the applicable steel strip is 0.18-0.30mm.

3. The method according to claim 1, characterized in that: The components and weight percentages of the applicable steel are: C: 0.04%-0.08%, Si: 3.0%-3.4%, Mn: 0.06%-0.12%, S: 0.01%-0.03%, Als: 0.02%-0.03%, N: 0.006%-0.01%, and the balance is Fe and unavoidable impurities.

4. According to the method described in claim 1, the molten steel is smelted in a converter and continuously cast, the ingot is heated to 1100-1250°C, and after conventional hot rolling, normalizing annealing is performed, and then cold rolling is performed to a finished product thickness of 0.18-0.30 mm; decarburization annealing, nitriding annealing, coating of magnesium oxide annealing isolation agent, high temperature annealing are performed, and after being taken out of the furnace, it is subjected to a stretching and flattening process, coating of an insulating coating, flattening and stretching annealing, and laser scoring.

5. According to the method of claim 1, the laser scoring equipment is arranged after the steel plate comes out of the flat stretching annealing furnace and before the online iron loss measuring instrument, and the steel plate is coiled into a finished oriented silicon steel coil after laser scoring.

Citation Information

Cited By

  • High-magnetic-induction oriented electrical steel and annealing process thereof

    CN120683427A

  • A high magnetic induction oriented electrical steel and its annealing process

    CN120683427B