A method for surface modification of short-cut polyethylene fibers and its products

By modifying the surface of ultra-high molecular weight polyethylene fibers to form a hydrophilic coating, the problem of poor dispersion of fibers in concrete is solved, the flowability and structural strength of concrete are significantly improved, and efficient fiber reinforcement effect is achieved.

CN115948915BActive Publication Date: 2024-11-22GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310007988.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-11-22
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

In the prior art, ultra-high molecular weight polyethylene fibers are poorly dispersed in concrete, resulting in less significant enhancement effect of concrete performance and significantly reduced working performance. This is mainly due to the hydrophobicity of the fiber surface, which makes it difficult for fibers to effectively disperse and mix in concrete.

Method used

The surface modification method of chopped polyethylene fibers was used to modify the fiber surface using polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) to change the fiber surface from hydrophobicity to virility Water-based, by controlling the concentration and temperature of P123, a thin hydrophilic coating is formed, improving the dispersion and flowability of the fibers in the concrete.

Benefits of technology

The modified fibers show significant fluidity improvement in concrete, and the ductility and structural strength of concrete have been significantly improved. The fluidity is increased by 89%-92%, and the tensile strength remains at 11.0-13.5MPa, satisfying the construction and Performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115948915B_ABST
    Figure CN115948915B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for surface modification of short-cut polyethylene fibers and its products, wherein the fiber surface modification method comprises the following steps: (1) first dissolving a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in an organic solvent at a mass ratio of 0.1%-5%; heating to 50-75°C, stirring continuously, so that the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is fully dissolved in the organic solvent; (2) after the dissolution is completed, adding short-cut polyethylene fibers, and stirring is maintained during the addition process; (3) after all the short-cut polyethylene fibers are added, the temperature is raised to 75-85°C and the solution is stirred continuously until the organic solvent is volatilized and removed; (4) the polyethylene fibers are taken out of the container, naturally air-dried or dried at 30-60°C in a drying oven for 1-24 hours, and the residual organic solvent is evaporated and removed. The method has easy-to-obtain process raw materials, simple operation, and very few steps, so that the surface of the ultra-high molecular weight polyethylene staple fiber changes from hydrophobic to hydrophilic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to engineering material pretreatment, in particular to a method for modifying the hydrophilicity of a fiber surface. The modified fiber material can be used for ultra-high ductility concrete, and belongs to the field of engineering fiber products. Background Art

[0002] Ultra-high ductility concrete is a fiber-reinforced composite material based on cement, quartz sand, etc., which uses high-ductility fiber materials and concrete to form a high-ductility structure at the microscopic level. It is also called "bendable concrete" because of its high ductility, high damage resistance, high tensile strength, and good crack self-suppression ability. The application of high-ductility concrete to buildings in various special environments can effectively improve the integrity of masonry houses, and is of great significance for enhancing the bearing capacity, ductility and crack resistance of masonry structures of buildings.

[0003] Ultra-high ductility concrete made of fiber is made by adding extremely strong tensile fibers into fresh concrete, so that the concrete has strong tensile and bending capabilities and extremely strong ductility. In the prior art, polypropylene coarse fibers, polyvinyl alcohol fibers, polypropylene microfibers, etc. are mainly added. Among them, ultra-high molecular weight polyethylene fibers are the commonly used fiber materials for ultra-high ductility concrete. The tensile strength of ultra-high molecular weight polyethylene fibers can reach 3000Mpa. A small amount of ultra-high molecular weight polyethylene fibers can achieve a significant improvement in the ductility and tensile resistance of concrete structures.

[0004] Conventional ultra-high molecular weight polyethylene fibers have a strong hydrophobic surface due to their large molecular weight. They are prone to curling and agglomeration during concrete mixing, which makes it difficult to effectively disperse fiber materials in ultra-high ductility concrete, resulting in a large deviation from theoretical expectations in terms of structural strength enhancement and concrete ductility improvement. In addition, due to the hydrophobicity of the polyethylene fiber surface, the polyethylene fiber has poor fluidity in fresh cement slurry, making fresh concrete difficult to mix and having poor working performance, especially not conducive to pumping. Summary of the invention

[0005] The purpose of the present invention is to provide a surface modification method and product of chopped polyethylene fibers to address the problems in the prior art that the hydrophobicity of the fiber surface leads to poor dispersion in high ductility concrete, insignificant concrete performance enhancement effect, and greatly reduced concrete working performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A method for surface modification of chopped polyethylene fibers comprises the following steps:

[0008] (1) First, dissolve the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in an organic solvent at a mass ratio of 0.1%-5%; heat to 50-75° C. and continue stirring to fully dissolve the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in the organic solvent.

[0009] (2) After the solution is completely dissolved, add the chopped polyethylene fibers and keep stirring during the addition process.

[0010] (3) After all the chopped polyethylene fibers are added, the temperature is raised to 75-85°C and the solution is continuously stirred until the organic solvent is evaporated and removed.

[0011] (4) The polyethylene fiber is taken out of the container and dried naturally or in a drying oven at 30-60° C. for 1-24 hours to evaporate and remove the residual organic solvent.

[0012] The method of the present invention is the modification and application of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123 for short) on the surface of short-cut polyethylene fibers, which changes the fiber surface from hydrophobic to hydrophilic, which is more economical and easier to implement than the traditional modification method. By controlling the concentration of P123 in the organic solution, the thickness of the hydrophilic coating on the fiber surface can be controlled, and only a thin layer of hydrophilic coating is evenly combined on the surface, without changing the fiber diameter, and the effect on the mechanical properties of the fiber is minimal. The process raw materials of this method are easy to obtain, the operation is simple, and the steps are minimal. The surface of the modified ultra-high molecular weight polyethylene staple fiber is wrapped by polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer. The polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is actually an active agent, the propylene oxide block is hydrophobic, and the ethylene oxide block is a hydrophilic head group. The hydrophobic side of P123 combines with the polyethylene staple fiber, and the hydrophilic side becomes a new fiber surface, ultimately changing the surface of the ultra-high molecular weight polyethylene staple fiber from hydrophobic to hydrophilic.

[0013] In the preparation method of the present invention, the heating temperature of the evaporated volatile organic solvent (anhydrous ethanol) is between 75-85 degrees Celsius, and the hydrophilic P123 is fully dispersed in the organic solvent. After the solvent is evaporated and released, P123 adheres to the polyethylene fiber surface to form a very thin and dense hydrophilic layer. When the solution temperature is higher than 85 degrees Celsius, the organic solvent is flammable, which increases the degree of danger. When it is lower than 75 degrees Celsius, the evaporation rate of the organic solvent is greatly reduced, so that the duration of the process is increased, affecting the economic cost. Therefore, for the preparation method of the present invention, it is the best choice to select a temperature of 75-85 degrees Celsius to form the hydrophilic layer on the fiber surface. In addition, the evaporation volatilization temperature affects the continuity and density of the surface hydrophilic film layer, which has a certain influence on the working performance of the final modified fiber in concrete. Selecting a suitable temperature is of great significance for better achieving the purpose of modification.

[0014] Finally, after the modified fiber of the present invention is applied to ultra-high ductility concrete, the fiber surface has good hydrophilicity, the surface modification layer is thin, and the fiber has excellent fluidity in the concrete. After the concrete solidifies, the ductility test results show that the chopped polyethylene fiber has the greatest improvement in concrete ductility. Moreover, due to the extremely thin surface hydrophilic layer, the strength of the polyethylene fiber is basically not reduced, and the overall strength of the concrete structure is good.

[0015] Furthermore, a hydrophilic layer with a thickness of 0.05-0.2 μm, preferably 0.1 μm, is formed on the surface of the chopped polyethylene fibers. The thinner hydrophilic film structure has the advantages of good adhesion, and the structural reinforcement effect of the modified polyethylene fibers in concrete is not affected.

[0016] Furthermore, the molecular weight of the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is 4000-9000. P122, P103, and P104 can be used instead of P123 as the raw material of the surface modification reagent.

[0017] Furthermore, the short-cut polyethylene fibers are fibers made of ultra-high molecular weight polyethylene. Preferably, the polyethylene fibers are fibers spun from polyethylene with a molecular weight of 1 million to 5 million.

[0018] Furthermore, the length of the chopped polyethylene fibers is 2-40 mm, preferably 3-20 mm.

[0019] Furthermore, the organic solvent in step (1) is a polar organic solvent, preferably a small molecule alcohol solution, such as methanol, ethanol, propanol, butanol, etc. Small molecule alcohols have the characteristics of good dissolution effect and easy evaporation and removal, and are used for polyethylene fiber surface modification with the advantages of low cost and high efficiency.

[0020] More preferably, the organic solvent is anhydrous ethanol.

[0021] When dissolving polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, anhydrous ethanol is selected. Anhydrous ethanol is volatile and inexpensive, which has obvious advantages over other organic solvents.

[0022] Furthermore, the amount of the short-cut polyethylene fibers added in step (2) is calculated based on the weight of the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer dissolved in step (1), and the weight of the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is 0.1%-5%, preferably 0.5%-2%, of the short-cut polyethylene fibers.

[0023] Furthermore, in step (2), the stirring speed is 5-100 r / min, preferably 5-30 r / min, and the chopped polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution by stirring.

[0024] Furthermore, the temperature in step (3) is preferably 78-82°C, such as 80°C.

[0025] Furthermore, in step (4), after the short-cut polyethylene fibers are heated and stirred to volatilize and remove the organic solvent, a very small amount of organic solvent will adhere to the fiber surface. Through further active drying or natural drying, the residual solvent is evaporated to achieve a fully firm combination of the surface-modified P123 and the short-cut polyethylene fibers.

[0026] The modified polyethylene fiber product is prepared by the above method.

[0027] Compared with the prior art, the solution of the present invention has the following beneficial effects:

[0028] 1. The chopped polyethylene fiber of the present invention is modified by polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), and the material has good adaptability and can be easily made into a polyethylene fiber surface coating, thereby greatly improving the hydrophilicity of the fiber.

[0029] 2. The modification method of the present invention adopts polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer to be dissolved in anhydrous ethanol solution to modify short-cut polyethylene fibers in the anhydrous ethanol solution. There is a difference between the temperature for controlling the dissolution of P123 and the temperature for high-temperature evaporation of the organic solvent (anhydrous ethanol) to form a surface coating. First, solid P123 is added to anhydrous ethanol at a relatively low temperature for dissolution to prevent the sputtering of the high-temperature organic solvent, and then the reaction temperature is increased to evaporate the organic solvent. P123 can be added to the organic solvent in a relatively safe environment. After the short-cut polyethylene fibers are completely added, the organic solvent is heated and evaporated, and the modification treatment of the polyethylene fiber performance is quickly completed, saving process time.

[0030] 3. The modification method of the present invention forms a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer coating with a thickness of about microns on the surface of the short-cut polyethylene fiber by evaporating the organic solvent and retaining the solute. The fiber has good hydrophilicity improvement effect, good fiber dispersion in fresh concrete, and outstanding effect on improving the fluidity of concrete.

[0031] 4. The surface of the chopped polyethylene staple fibers modified by the modification method of the present invention has good hydrophilicity. When the unmodified chopped polyethylene staple fibers are added to fresh concrete, the fluidity of the concrete will be significantly reduced, or even have no fluidity and cannot be used for construction. The concrete slump test shows that the polyethylene staple fibers modified by the patent method can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene staple fibers; the concrete J-ring expansion test shows that the polyethylene staple fibers modified by the patent method can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene staple fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a scanning electron microscope image (surface scan) of the cross section of the polyethylene fiber after surface modification.

[0033] Figure 2a It is the EDS spectrum (surface scan) of the cross section of polyethylene fiber after surface modification and the carbon element scan.

[0034] Figure 2b It is the EDS energy spectrum (surface scan) of the cross section of polyethylene fiber after surface modification and the oxygen element scan.

[0035] Figure 3 This is a scanning electron microscope image (line scan) of the cross section of the polyethylene fiber after surface modification.

[0036] Figure 4 This is the EDS spectrum (line scan) of the cross section of polyethylene fiber after surface modification. DETAILED DESCRIPTION

[0037] In order to better illustrate the technical solution of the present invention, the following is a detailed description in conjunction with specific implementation cases and test result data. It should not be considered that all descriptions are specific limitations on the present invention. All solutions implemented using the same inventive concept are within the scope of protection required by the present invention.

[0038] Example 1

[0039] A method for surface modification of polyethylene fibers comprises the following steps:

[0040] (1) First, dissolve the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in anhydrous ethanol at a mass ratio of 1 wt%. The container of anhydrous ethanol can be a beaker. To ensure that the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is evenly dispersed in the ethanol solution, place the beaker containing anhydrous ethanol in an oil bath and heat it to 60° C. and continue stirring to allow the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer to fully dissolve in the anhydrous ethanol solution.

[0041] (2) After the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is completely dissolved in anhydrous ethanol, short-cut polyethylene fibers are added to the anhydrous ethanol solution, and stirring is maintained during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is such that the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is 1wt% compared to the short-cut polyethylene fibers (i.e., polyethylene fibers are added in an amount 100 times the weight of P123).

[0042] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred. The purpose of this stage is to evaporate the solvent and retain the solute. The anhydrous ethanol solution is continuously stirred until the anhydrous ethanol is completely evaporated, and only the polyethylene fibers with the P123 coating (film layer) on the surface remain in the container.

[0043] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber can be naturally air-dried for 12 hours to evaporate the remaining anhydrous ethanol, thereby obtaining the surface-modified polyethylene fiber.

[0044] The prepared surface modified polyethylene fibers were characterized.

[0045] (1) Scanning electron microscope scan results

[0046] The polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer used for coating contains oxygen, while polyethylene fiber is composed of carbon and hydrogen. This shows that SEM-EDS can be used for elemental surface scanning analysis to determine whether the outer layer of the fiber is coated with a substance containing oxygen. If so, it means that the fiber surface is coated with polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

[0047] SEM-EDS fiber cross-section scan: The original SEM image of the cross-section of the polyethylene fiber after surface modification is as follows Figure 1 As shown, Figure 1 The corresponding energy spectrum is as follows Figure 2a and Figure 2b As shown. Figure 2a The carbon element and Figure 2b The distribution of oxygen elements shows that there is a dense distribution of oxygen elements inside the fiber cross section, because polyethylene fiber is composed of carbon and hydrogen. In the outer circle of the fiber cross section, the concentration of oxygen elements is significantly increased, similar to a ring, indicating that it is a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer coating.

[0048] (2) Scanning electron microscope line scan results

[0049] Through line scanning, the results are as follows Figure 3 and Figure 4As shown in the figure, it can be found that the oxygen content on both sides of the fiber suddenly increases, which means that the line scan scans the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer coating. Figure 4 The width of the section where the oxygen content increases can be judged that the thickness of the coating is about 3 microns.

[0050] (3) Liquidity test

[0051] The prepared surface modified polyethylene fiber is applied to concrete preparation, with the addition amount of 2wt% modified polyethylene fiber or 2wt% unmodified original polyethylene fiber, and C40 concrete is selected as the basic concrete formula. After the concrete slurry is prepared, the slump and J-ring expansion tests are carried out to compare the fluidity difference of the concrete slurry with modified polyethylene fiber and unmodified polyethylene fiber. The fluidity change of the concrete with polyethylene fiber is calculated based on the concrete with unmodified polyethylene fiber. The formula for calculating the fluidity improvement ratio is as follows: ((concrete fluidity with modified polyethylene fiber added - concrete fluidity with unmodified polyethylene fiber added) / (concrete fluidity with unmodified polyethylene fiber added))×100%.

[0052] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.0MPa.

[0053] Example 2

[0054] A method for surface modification of polyethylene fibers comprises the following steps:

[0055] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0056] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 0.2% by weight relative to the weight of the short-cut polyethylene fibers.

[0057] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0058] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0059] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 61% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 74% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 6.7MPa.

[0060] Example 3

[0061] A method for surface modification of polyethylene fibers comprises the following steps:

[0062] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0063] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 0.8% by weight relative to the weight of the short-cut polyethylene fibers.

[0064] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0065] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0066] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 86% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 12.4MPa.

[0067] Example 4

[0068] A method for surface modification of polyethylene fibers comprises the following steps:

[0069] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0070] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 2% by weight relative to the weight of the short-cut polyethylene fibers.

[0071] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0072] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0073] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.2MPa.

[0074] Example 5

[0075] A method for surface modification of polyethylene fibers comprises the following steps:

[0076] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0077] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 4% by weight relative to the weight of the short-cut polyethylene fibers.

[0078] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0079] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0080] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 9.7MPa.

[0081] The experiments in Examples 2-5 mainly compare and analyze the effects of different P123 dosages on the modification effect. When the dosage of P123 relative to the polyethylene fiber is 0.8%-2%, the modification effect is better, and both the concrete fluidity after adding the fiber and the final tensile strength of the concrete are excellent. Compared with unmodified polyethylene fiber, the improved fluidity can make concrete easier to construct and greatly expand the scope of application.

[0082] Example 6

[0083] A method for surface modification of polyethylene fibers comprises the following steps:

[0084] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 0.5%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0085] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0086] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0087] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0088] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 93% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.2MPa.

[0089] Example 7

[0090] A method for surface modification of polyethylene fibers comprises the following steps:

[0091] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 2%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0092] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0093] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0094] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0095] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.4MPa.

[0096] Example 8

[0097] A method for surface modification of polyethylene fibers comprises the following steps:

[0098] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 3%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0099] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0100] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0101] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0102] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 12.4MPa.

[0103] Example 9

[0104] A method for surface modification of polyethylene fibers comprises the following steps:

[0105] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 4%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0106] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0107] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0108] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0109] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 93% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.8MPa.

[0110] Example 10

[0111] A method for surface modification of polyethylene fibers comprises the following steps:

[0112] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 6%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0113] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0114] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0115] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0116] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete samples with modified polyethylene short fibers were made into standard concrete test blocks, and their tensile strength was tested to be 10.5MPa.

[0117] Embodiment 11

[0118] A method for surface modification of polyethylene fibers comprises the following steps:

[0119] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 10%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0120] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0121] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0122] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0123] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.1MPa.

[0124] Examples 6-11 mainly compare and analyze the effects of different concentrations of P123 dissolved in anhydrous ethanol on performance. The results show that the concentration has little effect, but it is best to choose a concentration between 1% and 4%, especially a dissolution concentration of 1% to 4%. After P123 is fully dissolved, it is easier to obtain a uniform thin layer of surface modification on the polyethylene fiber surface, avoiding the loss of polyethylene fiber reinforcement due to a thicker modified layer.

[0125] Example 12

[0126] A method for surface modification of polyethylene fibers comprises the following steps:

[0127] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 55°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0128] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0129] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0130] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0131] The concrete slump test showed that the modified polyethylene short fibers could improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers could improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 12.4MPa.

[0132] Embodiment 13

[0133] A method for surface modification of polyethylene fibers comprises the following steps:

[0134] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 65°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0135] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0136] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0137] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0138] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 93% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 12.1MPa.

[0139] Embodiment 14

[0140] A method for surface modification of polyethylene fibers comprises the following steps:

[0141] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 75°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0142] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0143] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0144] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0145] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 93% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.8MPa.

[0146] Embodiment 15

[0147] A method for surface modification of polyethylene fibers comprises the following steps:

[0148] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 80°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0149] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0150] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0151] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0152] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.9MPa.

[0153] Example 16

[0154] A method for surface modification of polyethylene fibers comprises the following steps:

[0155] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 85°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0156] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0157] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0158] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0159] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.3MPa.

[0160] Examples 12-16 mainly compare the effect of temperature change on the results of dissolving P123 in anhydrous ethanol. The dissolving temperature only affects the volatilization loss of anhydrous ethanol, and has little effect on the hydrophilic modified thin layer on the surface of the final polyethylene fiber. Only when the dissolving temperature exceeds 80°C, a certain amount of volatilization loss of anhydrous ethanol occurs, which slightly affects the dispersibility. Therefore, when dissolving P123, the temperature should not be too high, and it is best to control it between 55-80°C, preferably between 55-75°C.

[0161] Embodiment 17

[0162] A method for surface modification of polyethylene fibers comprises the following steps:

[0163] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0164] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0165] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 75°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0166] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0167] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 92% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.4MPa.

[0168] Embodiment 18

[0169] A method for surface modification of polyethylene fibers comprises the following steps:

[0170] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0171] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0172] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 85°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0173] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0174] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.5MPa.

[0175] Embodiment 19

[0176] A method for surface modification of polyethylene fibers comprises the following steps:

[0177] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0178] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0179] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 90°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0180] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0181] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 87% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 11.9MPa.

[0182] Embodiment 20

[0183] A method for surface modification of polyethylene fibers comprises the following steps:

[0184] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0185] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0186] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 95°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0187] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0188] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 86% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 88% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 10.8MPa.

[0189] Examples 17-20 compare and analyze the effect of temperature on stirring and drying after adding chopped polyethylene fibers. The effect is small, mainly because after the temperature exceeds 90°C, ethanol evaporates faster and the safety risk increases. At the same time, some P123 molecules may be degraded, and the surface adhesion is reduced, which reduces the firmness of the polyethylene fiber surface film layer, thereby reducing the structural reinforcement effect of polyethylene fibers in concrete.

[0190] Examples 21-24

[0191] A method for surface modification of polyethylene fibers comprises the following steps:

[0192] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0193] (2) After P123 is completely dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1% by weight relative to the weight of the short-cut polyethylene fibers.

[0194] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0195] (4) Take the polyethylene fiber out of the container. A very small amount of anhydrous ethanol will adhere to the fiber surface. Use a drying oven to dry for 8 hours to evaporate the remaining anhydrous ethanol, and the surface-modified polyethylene fiber is obtained. The drying oven temperature is shown in the following table.

[0196]

[0197] The test results show that different drying oven temperatures have little effect on the volatilization and removal of residual anhydrous ethanol. A slightly higher temperature may be more conducive to the drying effect, thereby making the modified polyethylene fiber dispersion effect better and better meeting the preparation requirements of ultra-high performance concrete.

[0198] Embodiment 25

[0199] A method for surface modification of polyethylene fibers comprises the following steps:

[0200] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0201] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1.05% by weight relative to the weight of the short-cut polyethylene fibers.

[0202] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0203] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0204] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 12.7MPa.

[0205] Embodiment 26

[0206] A method for surface modification of polyethylene fibers comprises the following steps:

[0207] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0208] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1.1% by weight relative to the weight of the short-cut polyethylene fibers.

[0209] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0210] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0211] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 90% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.4MPa.

[0212] Embodiment 27

[0213] A method for surface modification of polyethylene fibers comprises the following steps:

[0214] (1) First, dissolve P123 in anhydrous ethanol at a mass ratio of 1%. The container for anhydrous ethanol can be a beaker. Place the beaker in an oil bath and heat it to 60°C while stirring continuously to allow P123 to fully dissolve in the anhydrous ethanol solution.

[0215] (2) After P123 is dissolved, add the short-cut polyethylene fibers to the anhydrous ethanol solution, and keep stirring during the addition process so that the short-cut polyethylene fibers can be quickly dispersed in the anhydrous ethanol solution. The amount of short-cut polyethylene fibers is calculated as follows: P123 is 1.15% by weight relative to the weight of the short-cut polyethylene fibers.

[0216] (3) After all the chopped polyethylene fibers are added to the anhydrous ethanol, the temperature of the oil bath is raised to 80°C and the solution is continuously stirred until all the anhydrous ethanol is evaporated and only the polyethylene fibers remain in the container.

[0217] (4) The polyethylene fiber is taken out of the container. A very small amount of anhydrous ethanol will adhere to the surface of the fiber. The fiber is dried in a drying oven at 60° C. for 6 hours to evaporate the remaining anhydrous ethanol, thereby obtaining a surface-modified polyethylene fiber.

[0218] The concrete slump test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 89% compared with the unmodified polyethylene short fibers; the concrete J-ring expansion test showed that the modified polyethylene short fibers can improve the concrete fluidity by up to 91% compared with the unmodified polyethylene short fibers. The concrete sample with the modified polyethylene short fibers was made into a standard concrete test block, and its tensile strength was tested to be 13.5MPa.

Claims

1. A method for surface modification of short-cut polyethylene fibers, characterized in that: The steps include: (1) first dissolving a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in an organic solvent at a mass ratio of 1% to 4%; the organic solvent is anhydrous ethanol; Heat to 50-75°C and continue stirring to fully dissolve the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer in the organic solvent; (2) After the dissolution is complete, add the chopped polyethylene fibers and keep stirring during the addition process; The amount of the short-cut polyethylene fibers added is calculated based on the weight of the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer dissolved in step (1), and the ratio between the two is as follows: the weight of the polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer is 0.2%-4% of the short-cut polyethylene fibers; (3) After all the chopped polyethylene fibers are added, the temperature is raised to 75-85°C and the solution is continuously stirred until the organic solvent is evaporated and removed; (4) Take the polyethylene fiber out of the container and dry it naturally or in a drying oven at 40-60°C for 1-24 hours to evaporate and remove the residual organic solvent.

2. A method for surface modification of chopped polyethylene fibers according to claim 1, characterized in that: A hydrophilic layer with a thickness of 0.05-0.2 μm is formed on the surface of the chopped polyethylene fibers.

3. The method for surface modification of chopped polyethylene fibers according to claim 1, characterized in that: Step (2) stirring speed 5-100r / min.

4. A method for surface modification of chopped polyethylene fibers according to claim 3, characterized in that: Step (2) stirring speed 5-30r / min.

5. The method for surface modification of chopped polyethylene fibers according to claim 1, characterized in that: The temperature of step (3) is 78-82°C.

6. A modified polyethylene fiber product prepared by the method for surface modification of chopped polyethylene fibers according to any one of claims 1 to 5.