Roller heat treatment process method of GCr19SiMnMo material
Through the heat treatment process of GCr19SiMnMo material, a lower bainite structure is formed, which solves the problem of high cost of high-hardenability high-carbon chromium bearing steel materials, achieves cost reduction and roller quality improvement, and has excellent wear resistance and impact resistance. toughness.
Patent Information
- Application Number
- CN202410907335.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the high-hardenability high-carbon chromium bearing steel 100CrMnMoSi8-4-6 material is expensive and has a long order cycle, resulting in high production costs. A heat treatment process suitable for domestic GCr19SiMnMo materials is needed to reduce costs and improve roller quality. quality.
GCr19SiMnMo material is used for cutting, annealing, turning, quenching and tempering of hot-rolled bars. Through isothermal salt bath cooling and high-temperature tempering, a lower bainite structure is formed to improve wear resistance and impact toughness and avoid rolling. Defects caused by contact between components during heat treatment.
The raw material procurement cost is reduced by 20%-30%. The obtained roller has a uniform spheroidized structure and high hardness. The wear resistance and contact fatigue life are equivalent to that of the martensite structure. The impact toughness is increased by more than 2 times and the roller life is improved. and reliability.
Smart Images

Figure CN118726735A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a roller heat treatment process method of a GCr19SiMnMo material. Background Art
[0002] The rolling elements used in extra-large bearings generally refer to tapered rollers and cylindrical rollers. When the effective diameter of the roller is greater than 80 mm and less than 110 mm, high-hardenability high-carbon chromium bearing steel is required. Generally, imported 100CrMnMoSi8-4-6 bearing steel is used. Due to the high price and long order cycle of imported 100CrMnMoSi8-4-6, the production cost is high. Domestic GCr19SiMnMo materials are now used for alternative processing. Therefore, a heat treatment process suitable for GCr19SiMnMo materials is urgently needed to reduce production costs and improve roller quality. Summary of the invention
[0003] The purpose of the present invention is to provide a heat treatment process suitable for GCr19SiMnMo material.
[0004] The roller heat treatment process of a GCr19SiMnMo material of the present invention is carried out according to the following steps:
[0005] 1. Cutting: Select GCr19SiMnMo hot-rolled bars and then cut them;
[0006] 2. Annealing: annealing the material segment obtained in step 1;
[0007] 3. Heat treatment: Turn the annealed material section to obtain rollers, and then place the rollers in a single layer with a spacing of 80-150mm between each roller; then perform pre-cleaning, preheat and dry after cleaning, quench under a protective atmosphere after drying, and then use salt bath cooling. The cooled rollers are transferred to an isothermal salt tank for isothermal treatment. The isothermal rollers are then cleaned for rust prevention and then tempered.
[0008] The beneficial effects of the present invention are:
[0009] 1. The raw materials are domestic high-hardenability high-carbon chromium bearing steel GCr19SiMnMo, which is delivered in hot-rolled bar form, replacing the imported high-carbon chromium bearing steel 100CrMnMoSi8-4-6, which is delivered in annealed and polished bar form. The raw material procurement cost is 20%-30% lower.
[0010] 2. After the domestically produced high-hardenability high-carbon chromium bearing steel GCr19SiMnMo of the present invention is cut into sections using a circular saw / band saw, it is annealed separately using a box-type furnace. The spheroidized structure after annealing is uniform and the hardness dispersion after annealing is small.
[0011] 3. The present invention requires that the rollers are placed on the tooling in a manner such that the spacing between the rollers can prevent the rollers from contacting each other when the tooling equipped with the rollers moves in the heat treatment heating furnace, thereby causing heat treatment soft spot defects and unqualified troostite in the core.
[0012] 4. The heat treatment method of the present invention is different from that of 100CrMnMoSi8-4-6 bearing steel. The original process obtains martensitic structure after heat treatment; the improved heat treatment process obtains lower bainitic structure. The wear resistance and contact fatigue life of the lower bainitic structure are equivalent to those of the conventional martensitic structure, but the impact toughness is more than 2 times higher than that of the tempered martensite. Moreover, after the lower bainite isothermal quenching, the roller surface presents compressive stress, thereby improving the roller life and reliability.
[0013] 5. Because the rollers in this size range are extra-large rollers, a high-temperature tempering is added after isothermal treatment to stabilize the bainite structure after isothermal treatment and ensure product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The metallographic structure after annealing at 500 times;
[0015] Figure 2 This is the metallographic structure of isothermal treatment at 500 times. DETAILED DESCRIPTION
[0016] Specific implementation method 1: In this implementation method, a roller heat treatment process method of GCr19SiMnMo material is carried out according to the following steps:
[0017] 1. Cutting: Select GCr19SiMnMo hot-rolled bars and then cut them;
[0018] 2. Annealing: annealing the material segment obtained in step 1;
[0019] 3. Heat treatment: Turn the annealed material section to obtain rollers, and then place the rollers in a single layer with a spacing of 80-150mm between each roller; then perform pre-cleaning, preheat and dry after cleaning, quench under a protective atmosphere after drying, and then use salt bath cooling. The cooled rollers are transferred to an isothermal salt tank for isothermal treatment. The isothermal rollers are then cleaned for rust prevention and then tempered.
[0020] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that a box-type spheroidizing annealing furnace is used for annealing in step 2, and the annealing process is as follows: heating temperature: 800±10°C, heating time: 240±10min, rapid cooling to 720°C with the furnace, isothermal temperature 720±10°C, isothermal time 240±10min, cooling to 500°C with the furnace, and then air cooling to room temperature. Others are the same as specific implementation method 1.
[0021] Specific implementation method three: This implementation method is different from specific implementation method one in that the cleaning after placement in step two is divided into cleaning agent cleaning and water cleaning, the cleaning temperature is 50-80°C, and the cleaning time for each step is 10-15 minutes. The rest is the same as specific implementation method one.
[0022] Specific implementation method 4: This implementation method is different from specific implementation method 1 in that the preheating and drying temperature in step 2 is 250-350° C. and the preheating and drying time is 10-15 minutes. The rest is the same as specific implementation method 1.
[0023] Specific implementation method 5: This implementation method is different from specific implementation method 1 in that the heating temperature of the quenching in step 2 is 890-910° C. and the heating time is 120-150 min. The rest is the same as specific implementation method 1.
[0024] Specific embodiment 6: This embodiment is different from the specific embodiment 1 in that the protective atmosphere is a mixed gas of nitrogen, methanol and propane. The rest is the same as the specific embodiment 1.
[0025] Specific implementation method 7: This implementation method is different from the specific implementation method 1 in that the salt temperature of the salt bath is 230-250°C, the water content in the salt bath is ≤1.2%, and the cooling time is 10-15 minutes. The rest is the same as the specific implementation method 1.
[0026] Specific embodiment 8: This embodiment is different from specific embodiment 1 in that the isothermal temperature is 230-250° C. and the isothermal time is 480-720 min. The rest is the same as specific embodiment 1.
[0027] Specific embodiment 9: This embodiment is different from the specific embodiment 1 in that the cleaning and rust prevention is firstly ultrasonically cleaned at a frequency of 28-30KHZ and a water temperature of 40-60°C; then foaming cleaning is performed at a water temperature of 40-60°C; and then alkaline water cleaning is performed at a water temperature of 20-50°C, wherein the alkaline water is a sodium nitrite aqueous solution with a mass concentration of 0.5-0.8%. The rest is the same as the specific embodiment 1.
[0028] Specific embodiment 10: This embodiment is different from specific embodiment 1 in that the tempering temperature is 230-240°C and the tempering time is 240min-300min. The rest is the same as specific embodiment 1.
[0029] The beneficial effects of the present invention are verified by the following experiments:
[0030] Example 1: A roller heat treatment process for GCr19SiMnMo material
[0031] 1. Cutting
[0032] The raw materials are electroslag remelted hot-rolled bars produced by Beiman Special Steel Co., Ltd., material: GCr19SiMnMo, diameter: 105mm, cut using a circular saw, section length: 103±0.5mm, burr-free, and with a smooth cut surface.
[0033] 2. Annealing
[0034] The material sections are annealed using Hangzhou Jinzhou periodic box-type spheroidizing annealing furnace; placement method: upright single-layer placement, the spacing between material sections is 50mm, the annealing heating temperature is 800±10℃, the heating time is 240±10min, the furnace is quickly cooled to 720℃, the isothermal temperature is 720±10℃, the isothermal time is 240±10min, and the furnace is slowly cooled to 500℃, and then air-cooled to room temperature after being taken out of the furnace. Figure 1 The metallographic structure after annealing at 500 times; Figure 1 It can be seen that the spheroidized structure after annealing is uniform and the carbides are evenly distributed.
[0035] 3. Turning
[0036] Use a lathe to process the material segments into qualified sizes according to the process drawings.
[0037] 4. Heat treatment
[0038] The heat treatment (quenching and tempering) of the rollers is processed using an 850 roller bottom salt bath bainite quenching production line with a protective atmosphere.
[0039] 4.1 Roller placement: upright single layer placement, with a distance of 100mm between each roller.
[0040] 4.2 Pre-cleaning of rollers: Pre-cleaning removes impurities such as cutting fluid, dust, oil, etc. remaining on the roller surface to ensure that the appearance color of the roller is consistent after quenching and tempering. Entering the pre-cleaning station, it is divided into cleaning agent cleaning and water cleaning. Cleaning temperature: 60°C, each cleaning time: 12 minutes; after cleaning, preheating and drying, preheating and drying temperature: 300°C, preheating and drying time: 12 minutes. The cleaning agent is a water-based metal cleaning agent produced by Nanjing Kerun Industrial Media Co., Ltd., model: KR-F400H;
[0041] 4.3 Quenching heating: Heating temperature: 890±5℃, Heating time: 130min; Protective atmosphere during heating: nitrogen + methanol + propane
[0042] 4.4 Cooling: Use salt bath cooling, the moving table moves up and down, the moving speed is 400mm / s, the salt tank stirring motor is started, the stirring motor speed is 500rpm, the salt temperature is 235±5℃, the water content in the salt bath is 0.6%, and the cooling time is 12min.
[0043] 4.5 Isothermal treatment: The rollers after cooling are immediately transferred to an isothermal salt bath for isothermal treatment. The isothermal temperature is 235±5℃ and the isothermal time is 600min. Figure 2 The metallographic structure of isothermal treatment under 500 times Figure 2 It can be seen that the roller obtains lower bainite structure after isothermal treatment.
[0044] 4.6 Cleaning and rust prevention: Ultrasonic cleaning, frequency 30KHZ, water temperature 50±5℃; foaming cleaning, water temperature 50±5℃; alkaline water cleaning, water temperature 30±5℃, the anti-rust component in the cleaning tank is sodium nitrite aqueous solution, the mass concentration is 0.6%.
[0045] 5. Tempering treatment:
[0046] The rust-proofed rollers are cleaned and transported to an air tempering furnace for tempering stabilization treatment. The tempering temperature is 235±5℃ and the tempering time is 260min.
[0047] 6. Detection after heat treatment
[0048] Metallographic structure: lower bainite structure + a small amount of retained austenite + evenly distributed fine residual carbides.
[0049] Hardness: Surface hardness: 60.5HRC; 3mm hardness: 60HRC; Core hardness: 59.5HRC; Impact value: 202J / cm 2 . Retained austenite content: 2.8%.
[0050] Comparative Example: Roller heat treatment process of 100CrMnMoSi8-4-6 material:
[0051] 1. Cutting
[0052] The raw materials are annealed and polished bars with an effective diameter greater than 80mm and less than 110mm, and are cut using a circular saw or a band saw.
[0053] 2. Turning
[0054] Use a lathe to process the material segments into qualified sizes according to the process drawings.
[0055] 3. Heat treatment
[0056] The heat treatment (quenching and tempering) of the rollers is carried out using a salt bath martensitic quenching production line with a protective atmosphere roller hearth furnace.
[0057] 3.1 Pre-cleaning of rollers: Pre-cleaning removes impurities such as cutting fluid, dust, oil, etc. on the roller surface to ensure that the appearance color of the roller is consistent after quenching and tempering. The rollers are placed on the tooling according to the process requirements and enter the pre-cleaning station, which is divided into cleaning agent cleaning and water cleaning. Cleaning temperature: 50-80℃, each cleaning time: 6-10min; drying after cleaning, drying temperature: 110-130℃, drying time: 6-10min.
[0058] 3.2 Quenching heating: Heating temperature: 870-890℃, heating time: 100-150min.
[0059] 3.3 Cooling: Use salt bath cooling, the moving table moves up and down, and the salt tank stirring motor starts to improve the salt cooling performance. Salt temperature: 160-190℃, water content in the salt bath: 0%-1.2%, cooling time: 6-10min.
[0060] 3.4 Air cooling: Air cooling time is 6-10min, and the roller surface temperature after air cooling is ≤40℃.
[0061] 3.5 Cleaning and rust prevention: Immersion cleaning, a total of three stations: 1. Ultrasonic cleaning, frequency 28-30KHZ, water temperature 50±5℃; 2. Foaming cleaning, water temperature 50±5℃; 3. Cold water cleaning, water temperature 8±2℃, the cold water station contains 0.5-0.8% concentration of sodium nitrite aqueous solution for rust prevention.
[0062] 3.6 Tempering: Use air tempering furnace for high temperature tempering. Tempering temperature: 230-250℃, tempering time: 360min-480min.
[0063] 4. Detection after heat treatment
[0064] Metallographic structure: tempered martensite + a small amount of residual austenite + evenly distributed fine residual carbides
[0065] Hardness: Surface hardness: 58~64HRC; 3mm hardness: 58~64HRC; Core hardness: 58~64HRC; Impact value: 108J / cm 2 ; Retained austenite content: less than 5%.
[0066] By comparison, it can be seen that the embodiment uses domestic GCr19SiMnMo material and adopts a new heat treatment process, which not only reduces the production cost but also improves the roller quality.
Claims
1. A roller heat treatment process for GCr19SiMnMo material, characterized in that The method proceeds as follows:
1. Cutting: Select GCr19SiMnMo hot-rolled bars and then cut them; 2. Annealing: annealing the material segment obtained in step 1; 3. Heat treatment: Turn the annealed material section to obtain rollers, and then place the rollers in a single layer with a spacing of 80-150mm between each roller; then perform pre-cleaning, preheat and dry after cleaning, quench under a protective atmosphere after drying, and then use salt bath cooling. The cooled rollers are transferred to an isothermal salt tank for isothermal treatment. The isothermal rollers are then cleaned for rust prevention and then tempered.
2. The roller heat treatment process of a GCr19SiMnMo material according to claim 1 is characterized in that In step 2, a box-type spheroidizing annealing furnace is used for annealing, and the annealing process is as follows: heating temperature: 800±10°C, heating time: 240±10min, rapid cooling to 720°C with the furnace, isothermal temperature 720±10°C, isothermal time 240±10min, cooling to 500°C with the furnace, and then air cooling to room temperature.
3. The roller heat treatment process of a GCr19SiMnMo material according to claim 1 is characterized in that Step 2: Pre-cleaning is divided into cleaning agent cleaning and water cleaning, cleaning temperature: 50-80℃, each cleaning time: 10-15min.
4. The roller heat treatment process of a GCr19SiMnMo material according to claim 1 is characterized in that Step 2: The preheating and drying temperature is 250-350°C, and the preheating and drying time is 10-15 minutes.
5. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that Step 2: Quenching heating temperature: 890-910°C, heating time: 120-150min.
6. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that The protective atmosphere was a mixture of nitrogen, methanol and propane.
7. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that The salt temperature of the salt bath is 230-250°C, the water content in the salt bath is ≤1.2%, and the cooling time is 10-15min.
8. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that Isothermal temperature: 230-250°C, isothermal time: 480-720min.
9. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that The cleaning and rust prevention method first performs ultrasonic cleaning at a frequency of 28-30KHZ and a water temperature of 40-60°C; then performs foaming cleaning at a water temperature of 40-60°C; and then performs alkaline water cleaning at a water temperature of 20-50°C, wherein the alkaline water is a sodium nitrite aqueous solution with a mass concentration of 0.5-0.8%.
10. The roller heat treatment process of GCr19SiMnMo material according to claim 1 is characterized in that Tempering temperature: 230-240℃; Tempering time: 240min-300min.