Method for preparing regenerated aluminum alloy through centrifugal separation and purification of waste aluminum

By using centrifugal separation and cyclone centrifugal separators combined with rotating injection refining methods in scrap aluminum recycling, the problem of low scrap aluminum impurity removal efficiency in the existing technology has been solved, and the rapid large-scale low-energy production of high-quality recycled aluminum alloys has been achieved. consumption preparation, improving separation efficiency and continuous operation performance.

CN118726751APending Publication Date: 2024-10-01INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410751526.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing scrap aluminum recycling and impurity removal technology is inefficient, resulting in resource waste and high energy consumption, and cannot meet economic needs. In particular, the gravity sedimentation method requires long-term static sedimentation, and cannot achieve rapid large-scale low-energy consumption preparation of high-quality recycled aluminum.

Method used

The centrifugal separation method is used to increase the density of metal impurities by adding modifiers, and a cyclonic centrifugal separator is used to achieve efficient separation of aluminum melt and impurity phases. Combined with rotary injection refining, high-quality recycled aluminum alloys are obtained to achieve continuous operate.

Benefits of technology

It significantly reduces the separation time, improves the separation efficiency and continuous efficiency, realizes the rapid large-scale low-energy consumption preparation of high-quality recycled aluminum alloy, and overcomes the problems of long time and low efficiency in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726751A_ABST
    Figure CN118726751A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing regenerated aluminum alloy through centrifugal separation and purification of waste aluminum, and belongs to the technical field of secondary resource recovery. The method comprises the following steps: (1) melting waste aluminum to obtain an aluminum melt; (2) adding a modifier into the aluminum melt obtained in the step (1), so that the modifier is combined with metal impurities in the waste aluminum to obtain a modified aluminum melt; (3) the modified aluminum melt obtained in the step (2) is subjected to rotational flow centrifugal separation, and purified overflow aluminum melt and underflow aluminum melt rich in impurity phases are obtained; and (4) the purified overflow aluminum melt obtained in the step (3) is subjected to rotary injection refining, the high-quality regenerated aluminum alloy is obtained, and the underflow aluminum melt rich in impurity phases serves as excess materials to be recycled. According to the method, separation of the aluminum melt and the impurity phase is achieved through the cyclone centrifugal effect, efficient impurity removal of the waste aluminum and continuous preparation of the regenerated aluminum alloy are synchronously achieved, and therefore the purpose of upgrading and recycling of the waste aluminum alloy is achieved. According to the method, aiming at the problems of difficulty in separation of multi-element impurities, low efficiency and high environmental cost in the waste aluminum recovery industry, a traditional electrolytic aluminum-doped recovery method is changed into a novel short-distance preparation method mainly based on impurity phase modification-cyclone centrifugal separation, and large-scale application of waste aluminum regeneration cycle is easy to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of secondary resource utilization, relates to a recycled aluminum and an impurity removal method, and in particular to a method for removing impurity phases in aluminum by centrifugal separation. Background Art

[0002] Aluminum has the advantages of easy processing, high specific strength, corrosion resistance, and high electrical and thermal conductivity. It has a wide range of applications and is widely used. It is widely used in aerospace, construction, transportation, electronic communications, national defense and military industries.

[0003] The impurities contained in scrap aluminum alloys mainly include two categories: metal impurities and non-metallic impurities. Iron is the largest harmful metal impurity in aluminum alloys. If the content exceeds the standard, it will form a flaky iron-rich phase in aluminum. The flaky iron-rich phase will reduce the toughness and elongation of aluminum, seriously deteriorate the processing performance of the product, and also have a great impact. When the iron element exceeds the standard, it will cause the aluminum alloy matrix to split; non-metallic impurities mainly come from the pollution of the recycling process of scrap aluminum alloys, including aluminum nitride, spinel, slag / molten salt, grain refiner, etc. Among them, Al4C3, MgAl2O3, and (Ti,V)B2 have a high proportion of inclusions, which seriously endanger the performance of aluminum alloys.

[0004] At present, the scrap aluminum recycling and impurity removal technology is mainly centered on the dilution method and gravity sedimentation method. The dilution method adds a large amount of raw aluminum to the remelted scrap aluminum to reduce the impurity phase content in the scrap aluminum, resulting in a large waste of resources; the gravity sedimentation method uses the density difference between the aluminum melt and the impurity phase to make the impurity phase settle to the bottom of the furnace chamber through static, thereby achieving physical separation of the melt and impurities. This method requires a long period of static sedimentation, resulting in low efficiency and low continuous operation performance, which cannot meet the economic needs, so a technological breakthrough is urgently needed.

[0005] It can be seen from this that how to reduce the resistance to impurity convergence, shorten the separation time, improve the continuous energy efficiency of the equipment, improve the separation efficiency, reduce the energy consumption of the recovery process, and realize the continuous operation of waste aluminum impurity removal and recycled aluminum preparation, so as to achieve the purpose of rapid, large-scale, low-energy preparation of high-quality recycled aluminum and aluminum alloys, has become a problem that technical personnel in this field urgently need to solve. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum, which method reduces the separation time as much as possible, improves the separation efficiency, improves the continuity efficiency, and realizes the continuous removal of impurity phases, thereby achieving the purpose of removing impurities from waste aluminum.

[0007] According to the technical solution provided by the present invention, a method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized by comprising the following steps:

[0008] (1) Melting waste aluminum to obtain aluminum melt;

[0009] (2) adding a modifier to the aluminum melt obtained in step (1) to combine the modifier with metal impurities in the scrap aluminum to obtain a modified aluminum melt;

[0010] (3) performing cyclone centrifugal separation on the modified aluminum melt obtained in step (2) to obtain a purified overflow aluminum melt and an underflow aluminum melt rich in impurity phases;

[0011] (4) The purified overflow aluminum melt obtained in step (3) is subjected to rotary spray refining to obtain high-quality recycled aluminum alloy, and the bottom flow aluminum melt rich in impurity phase is recovered as residual material.

[0012] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the waste aluminum used as raw material in step (1) includes any one or more combinations of waste cans, waste automobile parts, waste molds, waste internal combustion engine pistons, waste aircraft aluminum, aluminum frames, waste cables, waste aluminum wires, waste extruded profiles, machined aluminum chips, and aluminum plate scraps. Typical but non-limiting combinations include combinations of waste automobile parts, waste molds, waste cast aluminum pots and pans, and internal combustion engine pistons; combinations of waste aircraft aluminum and aluminum frames; combinations of waste household tableware and waste kettles; combinations of waste aluminum wires and waste cables; and combinations of waste extruded profiles, machined aluminum chips, and aluminum plate scraps.

[0013] Preferably, the temperature of the aluminum melt during the melting process is 10-300°C higher than the melting point of the scrap aluminum, for example, it can be 10°C, 50°C, 100°C, 150°C, 200°C, 250°C or 300°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the chemical modifier described in step (2) includes any one or more combinations of Mn, Cr, La, Ce, Be, Zr, Ni, B, B2O3, boride, sodium borate, potassium borate, aluminum-boron master alloy, aluminum-manganese master alloy, aluminum-chromium master alloy, aluminum-cerium master alloy, and aluminum-lanthanum master alloy; the modifier can be added in the waste aluminum melting furnace or in a separate insulation furnace. The addition of the modifier can ensure that the occurrence form of metal impurities is changed, so that the phase density of metal impurities is increased.

[0015] Preferably, the amount of the chemical modifier added is 0.1-2.0%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%.

[0016] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the modified aluminum melt described in step (3) enters a cyclone centrifugal device through a pump, which includes an electromagnetic pump and a mechanical pump.

[0017] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the cyclone centrifugal separation device described in step (3) is a cyclone centrifugal separator, and its structure includes a feed pipe, a cyclone column section, a cyclone cone section, an overflow pipe and an underflow pipe.

[0018] Preferably, the diameter of the cyclone column section of the cyclone centrifugal separator is 0.05-0.5m.

[0019] Preferably, the height of the cyclone column section of the cyclone centrifugal separator is 0.7-2.0 times the diameter of the cyclone column section.

[0020] Preferably, the cone angle of the cyclone cone section of the cyclone centrifugal separator is 3-16°.

[0021] Preferably, the length-to-width ratio of the feed pipe of the cyclone centrifugal separator is 1.5:1-4:1.

[0022] Preferably, the equivalent diameter of the feed pipe of the cyclone centrifugal separator is 0.13-0.29 times the diameter of the cyclone column section.

[0023] Preferably, the diameter of the overflow pipe of the cyclone centrifugal separator is 0.2-0.4 times the diameter of the cyclone column section.

[0024] Preferably, the overflow pipe of the cyclone centrifugal separator is inserted into the cyclone column section to a depth of 0.2-1.0 times the diameter of the cyclone column section.

[0025] Preferably, the wall thickness of the overflow pipe of the cyclone centrifugal separator is 0.002-0.02 times the diameter of the cyclone column section.

[0026] Preferably, the diameter of the underflow pipe of the cyclone centrifugal separator is 0.1-0.2 times the diameter of the cyclone column section.

[0027] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the specific process of the cyclone centrifugal separation described in step (3) is: high-speed aluminum melt is pumped into the cyclone centrifugal separator, the cyclone causes the aluminum melt to produce a cyclone motion, the aluminum melt and the impurity phase are separated under the action of the cyclone, the purified aluminum melt flows out from the overflow port, and the impurity phase flows out from the bottom flow port along with a small part of the bottom flow aluminum melt, thereby achieving efficient separation of the aluminum melt and the impurity phase.

[0028] Furthermore, the impurity phase includes a chemically modified metal impurity phase and an unmodified non-metal impurity phase. The metal impurity phase includes iron and modifiers entrained in the scrap aluminum, and the non-metal impurity phase includes aluminum nitride, spinel, slag / molten salt, grain refiner and other inclusions mixed in the scrap aluminum recovery process.

[0029] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the temperature of the modified aluminum melt during the transmission process in step (3) is 10-300°C higher than the melting point of the waste aluminum, the flow rate of the transmitted modified aluminum melt is 1-15m / s, and the bottom flow diversion ratio of the cyclone centrifugal separator is 1%-50%.

[0030] As a further improvement of the present invention, the method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum is characterized in that the cyclone centrifugal separation system described in step (3) comprises a primary cyclone centrifugal separator, and a secondary cyclone centrifugal separator and a multi-stage cyclone centrifugal separator connected in series or in parallel.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The method provided by the present invention overcomes the continuous application of multiple units such as melt melting, melt transportation, online feeding, and melt impurity removal, and realizes the stable, efficient, and continuous preparation of high-quality recycled aluminum alloy.

[0033] (2) The method provided by the present invention is based on the in-situ modification of the impurity phase. By applying strong centrifugal force to accelerate the separation of the impurity phase and the melt, efficient and synchronous impurity removal of scrap aluminum is achieved, overcoming the common problems of the current gravity sedimentation method of removing impurities, such as long time, low efficiency and incomplete impurity removal. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The process flow chart of the present invention is

[0035] Figure 2 A typical route map of the process flow of the present invention is shown in FIG. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below by specific implementation schemes. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0037] Example 1

[0038] The present invention provides a method for preparing recycled aluminum by cyclonic centrifugal impurity removal, the method comprising the following steps:

[0039] (1) Figure 2 As shown, the scrap aluminum used as the raw material has an aluminum content of 95.2%, a magnesium content of 2.5%, a silicon content of 0.9%, an iron content of 1.1%, and a non-metallic impurity content of 9150mm 2 / kg, add it to the melting and modification furnace, the addition amount is 100kg, raise the temperature to 850℃, wait until the solid waste aluminum material is completely melted; add 1kg of modifier Mn to the melting and modification furnace, start stirring to mix the melt in the furnace evenly;

[0040] (2) The electromagnetic pump pumps the aluminum melt in the insulation molten pool into a cyclone separator with a cyclone column section diameter of 0.4 m at a speed of 8 m / s; after centrifugal separation, it enters the overflow insulation molten pool, and after rotary blowing refining, an aluminum melt with an iron content of 0.12% is obtained, and the removal rate of non-metallic impurities is 86.8%.

[0041] The specific composition of the recycled aluminum alloy obtained in this example is shown in Table 1.

[0042] Example 2

[0043] The present invention provides a method for preparing recycled aluminum by cyclonic centrifugal impurity removal, the method comprising the following steps:

[0044] (1) Figure 2 As shown, the scrap aluminum used as the raw material has an aluminum content of 94.3%, a magnesium content of 2.2%, a silicon content of 1.3%, an iron content of 0.5%, and a non-metallic impurity content of 6550mm 2 / kg, add it into the melting and modification furnace, the addition amount is 100kg, raise the temperature to 800℃, wait until the solid waste aluminum material is completely melted; add 2kg of modifier KBF4 into the melting and modification furnace, start stirring to mix the melt in the furnace evenly;

[0045] (2) The electromagnetic pump pumps the aluminum melt in the insulation molten pool into a cyclone separator with a cyclone column section diameter of 0.4 m at a speed of 5 m / s; after centrifugal separation, it enters the overflow insulation molten pool, and after rotary blowing refining, an aluminum melt with an iron content of 0.15% is obtained, and the removal rate of non-metallic impurities is 85.9%.

[0046] The specific composition of the recycled aluminum alloy obtained in this example is shown in Table 1.

[0047] Example 3

[0048] The present invention provides a method for preparing recycled aluminum by cyclonic centrifugal impurity removal, the method comprising the following steps:

[0049] (1) Scrap aluminum as raw material, with aluminum content of 94.9%, magnesium content of 2.4%, silicon content of 1.1%, iron content of 1.8%, non-metallic impurities content of 1420mm 2 / kg, add 80kg into the melting furnace, raise the temperature to 760℃, and wait until the solid waste aluminum material is completely melted;

[0050] (2) adding aluminum melt and 1.5 kg of modifier Mn into a separately provided modification furnace and stirring and mixing them uniformly;

[0051] (3) The electromagnetic pump pumps the aluminum melt in the modification furnace into a cyclone separator with a cyclone column section diameter of 0.4 m at a speed of 5 m / s; after centrifugal separation, it enters the overflow insulation molten pool, and after rotary blowing refining, an aluminum melt with an iron content of 0.23% is obtained, and the removal rate of non-metallic impurities is 93.1%.

[0052] The specific composition of the recycled aluminum alloy obtained in this example is shown in Table 1.

[0053] Example 4

[0054] The present invention provides a method for preparing recycled aluminum by cyclonic centrifugal impurity removal, the method comprising the following steps:

[0055] (1) Scrap aluminum as raw material, with aluminum content of 87.8%, magnesium content of 2.6%, copper content of 1.4%, zinc content of 4.6%, iron content of 2.1%, non-metallic impurities content of 1420mm 2 / kg, add 80kg into the melting furnace, raise the temperature to 760℃, and wait until the solid waste aluminum material is completely melted;

[0056] (2) adding aluminum melt and 0.8 kg of modifier Ce into a separately provided modification furnace and stirring and mixing them uniformly;

[0057] (3) The electromagnetic pump pumps the aluminum melt in the modification furnace into a cyclone separator with a cyclone column section diameter of 0.4 m at a speed of 6 m / s; after centrifugal separation, it enters the overflow insulation molten pool, and after rotary blowing refining, an aluminum melt with an iron content of 0.51% is obtained, and the removal rate of non-metallic impurities is 82.7%.

[0058] The specific composition of the recycled aluminum alloy obtained in this example is shown in Table 1.

[0059] Example 5

[0060] The present invention provides a method for preparing recycled aluminum by cyclonic centrifugal impurity removal, the method comprising the following steps:

[0061] (1) The scrap aluminum used as the raw material has an aluminum content of 85.7%, a copper content of 1.8%, a zinc content of 0.9%, a silicon content of 9.3%, an iron content of 2.5%, and a non-metallic impurity content of 5370 mm 2 / kg, add 80kg into the melting furnace, raise the temperature to 720℃, and wait until the solid waste aluminum material is completely melted;

[0062] (2) adding molten aluminum and 1 kg of modifier Ti into a separately provided modification furnace and stirring and mixing them uniformly;

[0063] (3) The electromagnetic pump pumps the aluminum melt in the modification furnace into a cyclone separator with a cyclone column section diameter of 0.4 m at a speed of 8 m / s; after centrifugal separation, it enters the overflow insulation molten pool, and after rotary blowing refining, an aluminum melt with an iron content of 0.76% is obtained, and the removal rate of non-metallic impurities is 91.2%.

[0064] The specific composition of the recycled aluminum alloy obtained in this example is shown in Table 1.

[0065] Table 1 Composition and content of recycled aluminum alloys in Examples 1-5

[0066] Example Fe content % Non-metallic impurities removal rate % Sample 1 0.12 86.8 Sample 2 0.15 85.9 Sample 3 0.23 93.1 Sample 4 0.51 82.7 Sample 5 0.76 91.2

[0067] Comparative Example 1

[0068] This comparative example provides a method for regenerating and removing iron from scrap aluminum, which adopts the method disclosed in Example 1 of CN117051248A, and specifically comprises the following steps:

[0069] (1) First, 20 tons of scrap aluminum are heated in a melting furnace to heat the scrap aluminum into aluminum melt, and the temperature of the aluminum melt reaches 700-750°C, which is the operating temperature of the aluminum melt in the iron removal process in the melting furnace.

[0070] (2) Then, magnesium oxide containing 2.148 times the amount of iron in the aluminum melt is introduced into the aluminum melt by compressed air; the amount of magnesium oxide used is 429.6 kg; magnesium oxide reacts with Fe and other elements in the liquid to form a composite oxide; wherein, the compressed air is supplied to the aluminum melt for the first 30 minutes at a speed of 20-50 L / min; the compressed air promotes the formation of Fe3O4 in the aluminum melt, which is then taken out of the aluminum melt by the composite oxide and removed by flotation filtration.

[0071] (3) 0.1-0.2% KCl-based refining agent is introduced into the aluminum melt by nitrogen, wherein the nitrogen is supplied to the aluminum melt for 30 minutes at a rate of 10-20 L / min; the nitrogen and the refining agent can clean up hydrogen and inclusions in the aluminum melt.

[0072] (4) Finally, the aluminum melt is filtered using a ceramic filter to separate the intermetallic compounds from the aluminum melt; the filtered aluminum melt can be directly used for casting aluminum materials such as aluminum rods.

[0073] Compared with Example 1, this comparative example requires an additional filtration step, which increases the processing cost. Although the prepared recycled aluminum achieves the removal of iron, it is far less than Example 1 and there is still much room for improvement.

[0074] It can be seen that the method provided by the present invention overcomes the difficulties in matching and connecting multiple units such as melt melting, melt transportation, online feeding, and melt impurity removal, and realizes the efficient, stable and continuous preparation of high-purity metal materials.

[0075] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing recycled aluminum alloy by centrifugal separation and purification of waste aluminum, characterized in that: The method comprises the following steps: (1) Melting waste aluminum to obtain aluminum melt; (2) adding a modifier to the aluminum melt obtained in step (1) to combine the modifier with metal impurities in the scrap aluminum to obtain a modified aluminum melt; (3) performing cyclone centrifugal separation on the modified aluminum melt obtained in step (2) to obtain a purified overflow aluminum melt and an underflow aluminum melt rich in impurity phases; (4) The purified overflow aluminum melt obtained in step (3) is subjected to rotary spray refining to obtain high-quality recycled aluminum alloy, and the bottom flow aluminum melt rich in impurity phase is recovered as residual material.

2. The method according to claim 1, characterized in that The waste aluminum used as the raw material in step (1) includes any one or more combinations of waste cans, discarded automobile parts, waste molds, discarded internal combustion engine pistons, waste aircraft aluminum, aluminum frames, waste cables, waste aluminum wires, waste extruded profiles, machined aluminum chips, and aluminum plate scraps. Typical but non-limiting combinations include combinations of waste automobile parts, waste molds, waste cast aluminum pots and pans, and internal combustion engine pistons; combinations of waste aircraft aluminum and aluminum frames; combinations of waste household tableware and waste kettles; combinations of waste aluminum wires and waste cables; and combinations of waste extruded profiles, machined aluminum chips, and aluminum plate scraps.

3. The method according to claim 1, characterized in that The chemical modifier described in step (2) includes any one or more combinations of Mn, Cr, La, Ce, Be, Zr, Ni, B, B2O3, borides, sodium borate, potassium borate, aluminum-boron master alloy, aluminum-manganese master alloy, aluminum-chromium master alloy, aluminum-cerium master alloy, and aluminum-lanthanum master alloy.

4. The method according to claim 1, characterized in that: The adding step of the modifier described in step (2) is included in an induction furnace, a resistance furnace, an arc furnace or a reverberatory furnace.

5. The method according to claim 1, characterized in that The device for cyclone centrifugal separation described in step (3) is a cyclone centrifugal separator, and its structure includes a feed pipe, a cyclone column section, a cyclone cone section, an overflow pipe and an underflow pipe. Preferably, the diameter of the cyclone column section of the cyclone centrifugal separator is 0.05-0.5m. Preferably, the height of the cyclone column section of the cyclone centrifugal separator is 0.7-2.0 times the diameter of the cyclone column section. Preferably, the cone angle of the cyclone cone section of the cyclone centrifugal separator is 3-16°. Preferably, the length-to-width ratio of the feed pipe of the cyclone centrifugal separator is 1.5:1-4:

1. Preferably, the equivalent diameter of the feed pipe of the cyclone centrifugal separator is 0.13-0.29 times the diameter of the cyclone column section. Preferably, the diameter of the overflow pipe of the cyclone centrifugal separator is 0.2-0.4 times the diameter of the cyclone column section. Preferably, the overflow pipe of the cyclone centrifugal separator is inserted into the cyclone column section to a depth of 0.2-1.0 times the diameter of the cyclone column section. Preferably, the wall thickness of the overflow pipe of the cyclone centrifugal separator is 0.002-0.02 times the diameter of the cyclone column section. Preferably, the diameter of the underflow pipe of the cyclone centrifugal separator is 0.1-0.2 times the diameter of the cyclone column section.

6. The method according to claim 1, characterized in that The modified aluminum melt described in step (3) enters the cyclone centrifugal device through a pump, which includes an electromagnetic pump and a mechanical pump.

7. The method according to claim 1, characterized in that The temperature of the modified aluminum melt during the transmission process in step (3) is 10-300°C higher than the melting point of the waste aluminum, the flow rate of the transmitted modified aluminum melt is 1-15m / s, and the bottom flow diversion ratio of the cyclone centrifugal separator is 1%-50%.

8. The method according to claim 1, characterized in that: The cyclone centrifugal separation system described in step (3) comprises a primary cyclone centrifugal separator, a secondary cyclone centrifugal separator and a multi-stage cyclone centrifugal separator connected in series or in parallel.