Additive manufacturing nanoparticle reinforced aluminum-based powder and preparation method thereof
By coating nano-TiC ceramic particles with high-energy ball milling and combining with low-energy ball milling, the problem of poor wettability and uneven distribution of nano-ceramic particles and aluminum matrix is solved, and the uniform distribution and interface bonding of nano-particles in aluminum-based composite materials are achieved. , improving the comprehensive performance of 3D printed aluminum matrix composite materials.
Patent Information
- Application Number
- CN202411036674.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the physical property differences between the nanoceramic particles and the aluminum matrix lead to poor wettability and weak interfacial bonding, which limits the content of the reinforcing phase and is prone to defects. In addition, the huge specific surface area of the nanoceramic particles results in the formation of composite materials. Uneven distribution and poor tissue uniformity affect material properties.
The aluminum alloy is fully coated on the nano-TiC ceramic particles through high-energy ball milling, and then low-energy ball milling is performed to evenly mix the aluminum alloy to ensure uniform distribution of the nano-TiC particles and avoid agglomeration, thereby improving the interface bonding strength.
It achieves uniform distribution and interface bonding of nanoparticles in aluminum-based composite materials, reduces processing defects, improves the overall performance and fluidity of the material, and meets the needs of 3D printing high-performance nanoparticle-reinforced aluminum-based composite materials.
Smart Images

Figure CN118726784A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal 3D printing, and in particular to a 3D printed nanoparticle-reinforced aluminum-based composite powder and a preparation method thereof. Background Art
[0002] 3D printing technology, also known as additive manufacturing technology, is a technology that directly forms and manufactures physical parts based on a three-dimensional CAD model designed by a computer. Unlike traditional subtractive manufacturing technology, 3D printing technology does not require tools such as knives, molds, and fixtures. It adopts a bottom-up layer-by-layer stacking manufacturing method with high forming accuracy. In recent years, additive manufacturing technology has developed rapidly and has received widespread attention from academia and industry around the world. Only one forming device is needed to produce various parts with complex structures, realizing personalized and liberalized production, greatly simplifying the forming process, reducing the processing cycle, and realizing the concept of net forming processing. It may become a disruptive technology in the fields of aerospace, defense industry, automobiles, and medical care. Laser additive manufacturing technology is a typical representative of metal additive manufacturing technology. It uses a high-energy laser beam as an energy source to melt metal raw materials such as powder, and then stacks them layer by layer to solidify them into a dense entity. Currently commonly used materials include Fe-based alloys, Ni-based alloys, Ti-based alloys, and Al-based alloys.
[0003] With the development of industry, single materials can no longer meet people's increasingly stringent demands for material performance, and composite materials have emerged. Nano-ceramic particle reinforced aluminum-based composite materials are favored by people because of their excellent properties such as low density, high specific strength, good wear resistance, and low thermal expansion coefficient. The use of 3D printing to form aluminum-based composite materials has unique advantages: on the one hand, complex parts can be directly integrated to simplify the processing technology; on the other hand, the high cooling rate in metal 3D printing can significantly refine the grain size of metal components and improve the comprehensive performance of the material. Powder preparation and its characteristics have a significant impact on the metal 3D printing forming process and forming quality. For 3D printing of nano-ceramic particle reinforced aluminum-based composite materials, it is usually necessary to first evenly mix the nano-ceramic reinforcement particles with the aluminum alloy powder, and then use a high-energy laser beam to melt the powder into shape. The current method for preparing ceramic particle reinforced aluminum-based nano-composite powders is generally to use low-energy ball milling to directly mix the reinforcement particles with the metal matrix. However, due to the difference in physical properties between the added ceramic particles and the aluminum matrix, the wettability is poor, the interface bonding is weak, the content of the reinforcement phase is limited, defects are easily generated during the forming process, and the strengthening effect is limited. In addition, the huge specific surface area of nano-ceramic particles makes it very easy for them to agglomerate under the action of van der Waals forces, resulting in uneven distribution of the formed composite material and poor organizational uniformity, which affects the material properties. Summary of the invention
[0004] In order to solve the defects of the prior art, the present invention aims to provide a method for preparing 3D printed nanoparticle-reinforced aluminum-based composite powder, which can effectively improve the wettability of the reinforcement phase with the matrix and maintain the uniform distribution of the reinforcement phase, thereby meeting the needs of 3D printing high-performance nanoparticle-reinforced aluminum-based nanocomposite components.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is: first, the aluminum alloy is fully coated on the nano-TiC ceramic particles by high-energy ball milling, and then the powder and the aluminum alloy are uniformly mixed by low-energy ball milling to obtain metal-coated nano-particle reinforced aluminum-based composite material powder.
[0006] The specific steps of the technical solution adopted by the present invention are as follows:
[0007] Step 1: Use spherical AlSi10Mg powder with a purity of 99.9% and a particle size of 18-45 μm and irregular TiC ceramic powder with a purity of 99.9% and a particle size of 60-100 nm;
[0008] Step 2, AlSi10Mg and TiC are weighed in a mass ratio of 4:1, mixed and placed in a high-energy ball mill for a long time, the ball mill speed is set to 300 rpm / min, the time is set to 10-15h, the grinding balls are selected as stainless steel balls, the ball-to-material ratio is selected to be 10:1, after high-energy ball milling, the ceramic particles are fully distributed inside the aluminum alloy powder, and the aluminum alloy powder is refined to obtain aluminum alloy-coated nano-TiC ceramic particles;
[0009] Step 3, the aluminum alloy coated TiC ceramic particles and AlSi10Mg powder are mixed in a mass ratio of 1:4, so that the total mass percentage of the nano-TiC particles is 5wt.%, and then put into a planetary ball mill for low-energy ball milling, the ball mill speed is set to 200rpm, the time is set to 4h, the grinding balls are selected as ceramic balls, and the ball-to-material ratio is selected as 2:1. After low-energy ball milling, the aluminum alloy coated nano-TiC ceramic particles and the AlSi10Mg powder are uniformly dispersed;
[0010] Step 4: Screen and grade the aluminum alloy-coated nano-TiC ceramic particle-reinforced aluminum-based composite powder obtained above to obtain a metal-coated nano-particle-reinforced aluminum-based composite powder for 3D printing with a desired particle size.
[0011] Compared with the prior art, the present invention mainly embodies the following advantages:
[0012] (1) The present invention provides an additively manufactured nanoparticle-reinforced aluminum-based powder and a preparation method thereof, which can ensure that nano-TiC particles are evenly distributed in the aluminum alloy body, and the aluminum alloy is coated on the nano-TiC particles to prevent the nano-particles from agglomerating, thereby strengthening the bonding with the matrix and reducing defects caused by poor wettability in subsequent processing. In addition, the particle size of the aluminum matrix powder can be reduced under the action of high-energy ball milling to avoid affecting the subsequent powder spreading process.
[0013] (2) The present invention provides an additive manufacturing nanoparticle-reinforced aluminum-based powder and a preparation method thereof, which, on the one hand, ensures uniform distribution of nano-TiC particles, and on the other hand, enables the AlSi10Mg powder to maintain a spherical shape, thereby ensuring the high fluidity and high bulk density required in the 3D printing process.
[0014] (3) The present invention provides an additive manufacturing nanoparticle-reinforced aluminum-based powder and a preparation method thereof, which combines the bonding properties of the reinforcement phase with the aluminum alloy and the machinability of the composite powder, and fully meets the requirements of 3D printing for high-performance nanoparticle-reinforced aluminum-based composite powders. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the low-magnification SEM morphology of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling in Example 1;
[0016] Figure 2 This is the high-magnification SEM morphology of the metal-coated nano-TiC particle composite powder for 3D printing obtained by high-energy ball milling in Example 1;
[0017] Figure 3 This is a high-magnification TEM image of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling in Example 1;
[0018] Figure 4 This is the low-magnification SEM morphology of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling in Example 2;
[0019] Figure 5 This is the high-magnification SEM morphology of the metal-coated nano-TiC particle composite powder for 3D printing obtained by high-energy ball milling in Example 2;
[0020] Figure 6 This is a high-magnification TEM image of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling in Example 2;
[0021] Figure 7 The low-magnification SEM morphology of the 3D printing-specific nano-TiC particle-reinforced aluminum alloy composite powder prepared by low-energy ball milling in the comparative example;
[0022] Figure 8 The high-magnification SEM morphology of the 3D printing-specific nano-TiC particle-reinforced aluminum alloy composite powder obtained by low-energy ball milling in the comparative example;
[0023] Fig. 9 This is a high-magnification TEM image of the 3D printing-specific nano-TiC particle-reinforced aluminum alloy composite powder prepared by low-energy ball milling in the comparative example. Specific implementation plan
[0024] In order to further illustrate the purpose and technical solution of the present invention, the present invention will be described in detail below in conjunction with specific implementation methods. Obviously, the implementation methods involved below are only for illustrating some embodiments of the present invention and do not limit the protection scope of the present invention.
[0025] A 3D printed nanoparticle-reinforced aluminum-based composite powder comprises an aluminum-based composite powder in which nano-TiC ceramic particles are uniformly dispersed and an aluminum alloy matrix without nano-TiC particles. In the present application, the aluminum alloy-coated nano-TiC particles have good interface bonding strength with the aluminum alloy matrix.
[0026] The preparation method of a 3D printed nanoparticle-reinforced aluminum-based composite powder described in the present application is: high-energy ball milling is used to uniformly disperse nano-TiC particles in the aluminum alloy, the aluminum alloy is fully coated on the surface of the nano-TiC particles, and then low-energy ball milling is used to uniformly mix the composite powder after high-energy ball milling with the aluminum alloy powder.
[0027] Example 1
[0028] (1) Spherical AlSi10Mg powder with a purity of more than 99.9% and a particle size of 18-45 μm and irregular TiC ceramic powder with a purity of more than 99.9% and a particle size of 60-100 nm are selected.
[0029] (2) Nano-TiC particles and AlSi10Mg powder with a mass ratio of 1:4 were weighed, mixed and placed in a single-tank planetary high-energy ball mill for high-energy ball milling. Argon was introduced to prevent the aluminum alloy from being oxidized. The ball milling speed was set to 300 rpm / min, the ball milling time was set to 5 hours, and the ball milling medium was selected as two stainless steel balls with different diameters, with diameters of 8 mm and 10 mm, respectively. The mass ratio of the two grinding balls was 1:1, and the ball-to-material ratio was selected as 10:1. In order to prevent the temperature from being too high during the ball milling process, a ball milling method of running for 15 min and then pausing for 5 min was adopted. After high-energy ball milling, the nano-TiC ceramic particles were evenly dispersed in the aluminum alloy powder, and the aluminum alloy powder was refined to obtain aluminum alloy-coated nano-TiC ceramic particles.
[0030] (3) The composite powder after high-energy ball milling and AlSi10Mg powder were weighed in a mass ratio of 1:4, mixed and placed in a single-tank planetary ball mill for low-energy ball milling, while argon gas was introduced for protection. The ball milling speed was set to 200 rpm / min, the ball milling time was set to 10 hours, and the ball milling media were selected as two ceramic balls with different diameters, with diameters of 8 mm and 10 mm, respectively. The mass ratio of these two grinding balls was 1:1, and the ball-to-material ratio was selected as 2:1. The ball milling method of running for 15 minutes and then pausing for 5 minutes was also selected. After low-energy ball milling, the aluminum alloy-coated nano-TiC ceramic particles and the AlSi10Mg powder were uniformly dispersed and maintained good fluidity and sphericity.
[0031] (4) The composite powder is screened using a 400-mesh sieve to filter out large particles of powder, thereby obtaining a uniform, fine, and highly fluid metal-coated nanoparticle-reinforced aluminum-based composite powder specifically for 3D printing.
[0032] The low-magnification and high-magnification SEM morphologies of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling are as follows: Figure 1 and Figure 2 As shown in the figure, it can be seen that after 10 hours of high-energy ball milling, the AlSi10Mg powder was broken and refined, and the average particle size was reduced to 5.74μm. The TiC particles were broken and refined. The high-magnification TEM image is shown in Figure 3 As shown, it can be seen that after 10 hours of high-energy ball milling, the nano-TiC particles gradually enter the interior of the aluminum alloy and achieve good interface bonding.
[0033] Example 2
[0034] This embodiment is the same as Specific Example 1 except that the high-energy ball milling time in step (2) is set to 15 hours.
[0035] The low-magnification and high-magnification SEM morphologies of the metal-coated nano-TiC particle composite powder for 3D printing prepared by high-energy ball milling are as follows: Figure 4 and Figure 5 As shown in the figure, it can be seen that after 15h of high-energy ball milling, the AlSi10Mg powder was significantly refined, with an average particle size of only 4.26μm. The high-magnification TEM image is shown in Figure 6 As shown, it can be seen that nano-TiC is uniformly dispersed inside the aluminum matrix, achieving good interface bonding.
[0036] Comparative Example
[0037] The present invention is a 3D printed nano-particle reinforced aluminum-based composite powder and a preparation method thereof. In order to further illustrate the outstanding advantages of the present invention, this comparative example is based on direct low-energy ball milling to prepare nano-TiC particle reinforced aluminum alloy composite powder, and its low-magnification and high-magnification SEM images are shown as follows: Figure 7 and Figure 8 As shown in the high magnification TEM image Fig. 9 As shown, it can be seen that after low-energy ball milling, the nano-TiC particles only adhere to the surface of the aluminum alloy powder and cannot achieve good interface bonding. The composite powder of the present application has a better effect.
[0038] Under appropriate processing conditions, uniform, fine, and highly fluid metal-coated nanoparticle-reinforced aluminum-based nanocomposite powders for 3D printing can be obtained, which can meet the requirements of metal 3D printing for the powder properties of composite powders, improve the wettability of ceramic particles to aluminum melt during processing, promote the uniform dispersion of ceramic particles in the matrix, enhance the interface bonding ability, and significantly improve the comprehensive performance of 3D printed aluminum-based composite components. The present invention adopts a method combining high-energy ball milling and low-energy ball milling to prepare metal-coated nanoparticle-reinforced aluminum-based composite powders for 3D printing, while combining the bonding properties of the reinforcing phase with the aluminum alloy and the machinability of the composite powder. The process is simple, efficient, and low-cost, and it is suitable for large-scale production of composite powders for 3D printing.
[0039] In summary, the current method for preparing ceramic particle reinforced nano-aluminum-based composite material powder is mainly to use low-energy ball milling to uniformly mix the reinforced particles with the metal matrix, but the powder nanoparticles obtained by this method will spontaneously agglomerate due to their huge specific surface area, and have poor wettability, and the interface bonding between the reinforced particles and the aluminum matrix is weak, which is prone to defects during the processing process, seriously affecting the performance of 3D printed aluminum-based composite material components. The metal-coated ceramic particle reinforced aluminum-based nanocomposite powder obtained by this invention has uniform nanoparticle distribution, strong interface bonding, and the aluminum alloy doped with nanoparticles has a small particle size, good fluidity, and consistent chemical composition, which can meet the demand for composite powders in metal 3D printing. The present invention innovatively uses a method combining high-energy ball milling and low-energy ball milling to prepare metal-coated ceramic particle reinforced aluminum-based nanocomposite powder for 3D printing, which saves production costs, improves production efficiency, and can achieve excellent comprehensive performance of 3D printed aluminum-based composite material components.
[0040] For those skilled in the art of metal 3D printing, it is obvious that the present invention is not limited to the details shown in the above-listed embodiments, and the results of the present invention can be obtained by other means without violating the innovation or core features of the present invention. Therefore, the above-mentioned embodiments are only exemplary explanations of the technical solutions of the present invention, and do not mean that the scope of protection of the present invention is limited thereto, and all changes and applications equivalent to those in the claims are included in the present invention.
Claims
1. A 3D printed nanoparticle-reinforced aluminum-based composite powder, characterized in that It includes fine aluminum-based powder doped with nano-TiC particles and pure aluminum alloy powder without nano-TiC particles.
2. The 3D printed nanoparticle-reinforced aluminum-based composite powder according to claim 1, characterized in that: The aluminum alloy is coated on the surface of the nano-TiC ceramic particles by high-energy ball milling, and the metal-coated ceramic particles are mixed with the aluminum alloy by low-energy ball milling, wherein the mass fraction of TiC is 5%.
3. A method for preparing a 3D printed nanoparticle-reinforced aluminum-based composite powder, comprising the following steps: Step 1: Use spherical AlSi10Mg powder with a purity of 99.9% and a particle size of 18-45 μm and irregular TiC ceramic powder with a purity of 99.9% and a particle size of 60-100 nm; Step 2: AlSi10Mg and TiC are weighed in a mass ratio of 4:1, mixed and placed in a high-energy ball mill for a long time, so that the ceramic particles are fully distributed inside the aluminum alloy powder after high-energy ball milling, and the aluminum alloy powder is refined to obtain aluminum alloy-coated nano-TiC ceramic particles; Step 3, the aluminum alloy coated TiC ceramic particles and AlSi10Mg powder are mixed in a mass ratio of 1:4, and then put into a planetary ball mill for low-energy ball milling. After low-energy ball milling, the aluminum alloy coated nano-TiC ceramic particles and AlSi10Mg powder are uniformly dispersed; Step 4: Screen and grade the aluminum alloy-coated nano-TiC ceramic particle-reinforced aluminum-based composite powder obtained above to obtain a metal-coated nano-particle-reinforced aluminum-based composite powder for 3D printing with a desired particle size.
4. The method for preparing a 3D printed nanoparticle-reinforced aluminum-based composite powder according to claim 3, characterized in that: In step 2, the ball milling speed is set to 300 rpm / min, the time is set to 10-15 h, the grinding balls are stainless steel balls, the ball-to-material ratio is selected to be 10:1, and argon gas is introduced for protection.
5. The method for preparing a 3D printed nanoparticle-reinforced aluminum-based composite powder according to claim 3, characterized in that: In step 3, the ball milling speed is set to 200 rpm / min, the time is set to 4 h, the grinding balls are selected as ceramic balls, the ball-to-material ratio is selected to be 2:1, and argon gas is introduced for protection.
Citation Information
Cited By
TiC particle reinforced aluminum alloy powder for metal 3D printing and preparation method of TiC particle reinforced aluminum alloy powder
CN119351829A
Nano-composite ceramic particle modified aluminum alloy powder for 3D printing and preparation method of nano-composite ceramic particle modified aluminum alloy powder