Aluminum alloy raised floor

By using aluminum alloy die-casting parts in the raised floor, which contain specific elements and are surface treated and hardened, the problem of insufficient structural strength of the raised floor is solved, high load-bearing capacity and lightness are achieved, and it is suitable for the needs of high-precision semiconductor factories. .

CN118726797APending Publication Date: 2024-10-01HUIYA ALUMINUM ALLOY PRODS SHANGHAI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310340541.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing raised floor's structural strength is insufficient and its load-bearing capacity is limited, which results in limited machine and equipment settings in high-precision semiconductor factories, and excessive materials waste resources and increase manufacturing costs.

Method used

It is made of aluminum alloy die castings, containing 7-11% silicon, 3-9% magnesium, 1-3% copper, and has a magnesium silicide phase. It is surface treated to form a free epoxy resin coating and nickel-chromium coating. Layer, powder coating, solid solution, quenching and aging treatment to improve strength.

Benefits of technology

It achieves the high load-bearing capacity, lightness, easy assembly and energy saving of the aluminum alloy elevated floor, and is suitable for factories with high-weight machine equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726797A_ABST
    Figure CN118726797A_ABST
Patent Text Reader

Abstract

An aluminum alloy raised floor is an aluminum alloy die casting, and the aluminum alloy die casting comprises 7-11 wt% of silicon, 3-9 wt% of magnesium, 1-3 wt% of copper and the balance aluminum, and the aluminum alloy die casting has a magnesium silicide (Mg2Si) phase. The aluminum alloy raised floor disclosed by the invention shows better yield strength and has excellent bearing capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an aluminum alloy elevated floor, and more particularly to an aluminum alloy elevated floor comprising an aluminum alloy with a specific composition. Background Art

[0002] The advantage of the raised floor is that there is a certain amount of suspended space between the raised floor surface where the equipment is placed and the ground. In addition to being used for laying out pipelines and facilitating construction by workers, exhaust equipment can also be installed to continuously remove the generated dust and prevent it from falling on the surface of products or parts. Currently, in various high-precision semiconductor factories, in order to facilitate the air quality of the clean environment, most of them are equipped with multiple micro-perforated raised floors to maintain the required environmental cleanliness to ensure that they meet the specifications of the clean room.

[0003] However, the structural strength of conventional elevated floors is often insufficient, and the limited load-bearing capacity restricts the installation of equipment. For example, when heavier equipment used in semiconductor processes is placed on the elevated floor, the elevated floor is prone to dents and cracks.

[0004] On the other hand, raised floors are often too heavy, which not only wastes materials but also increases manufacturing costs.

[0005] Therefore, the industry expects an elevated floor with excellent load-bearing capacity and light material. Summary of the invention

[0006] In view of the various deficiencies of the above-mentioned known technologies, the present disclosure provides an aluminum alloy elevated floor, which includes an aluminum alloy die-casting, and the aluminum alloy die-casting includes:

[0007] 7 to 11 wt % silicon;

[0008] 3 to 9% by weight of magnesium;

[0009] 1 to 3 wt. % copper; and

[0010] The balance of aluminum,

[0011] The aluminum alloy die casting has a magnesium silicide (Mg2Si) phase.

[0012] In at least one embodiment, the aluminum alloy elevated floor of the present disclosure is formed with through holes to serve as a honeycomb panel, a grille panel, or a window floor.

[0013] In at least one embodiment, the aluminum alloy elevated floor of the present disclosure is surface treated so that the surface of the aluminum alloy die casting is formed with at least one surface treatment layer selected from the group consisting of epoxy resin coating, nickel-chromium coating, powder coating, and anodizing.

[0014] In at least one embodiment, the aluminum alloy die casting comprises 7.5 to 9.5 weight % silicon. In at least one embodiment, the aluminum alloy die casting comprises 3.5 to 6.5 weight % magnesium. In at least one embodiment, the aluminum alloy die casting comprises 3.5 to 5.5 weight % magnesium or 4 to 6 weight % magnesium. In at least one embodiment, the aluminum alloy die casting comprises 1.5 to 2.5 weight % copper.

[0015] In at least one embodiment, the aluminum alloy die casting is an aluminum alloy die casting of modified ADC12. In at least one embodiment, the aluminum alloy die casting is made by die casting of ADC5 and ADC14.

[0016] In at least one embodiment, the density of the aluminum alloy die casting is 2.6 or more. In at least one embodiment, the tensile strength of the aluminum alloy die casting is 190 MPa or more. In at least one embodiment, the yield strength of the aluminum alloy die casting is 200 MPa or more.

[0017] In at least one embodiment, the aluminum alloy die casting is subjected to precipitation hardening treatment, wherein the precipitation hardening treatment includes solution treatment, quenching treatment and aging treatment.

[0018] In at least one embodiment, the solution treatment is heating the aluminum alloy die casting to 450 to 550° C. and maintaining at the temperature for 1.5 to 2 hours.

[0019] In at least one embodiment, the aging treatment is an artificial aging treatment.

[0020] In at least one embodiment, the artificial aging treatment is performed at 500° C. for 120 minutes.

[0021] The aluminum alloy elevated floor disclosed in the present invention is light in weight and can provide a high load-bearing capacity, is easy to assemble, saves labor, and saves energy, and is applicable to factories that need to install heavy-duty machines and equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figures 1 to 10 This is an electron microscope image of the aluminum alloy die casting embodiment 1 of the aluminum alloy elevated floor disclosed in the present invention, wherein: Figure 1 , 3 , 5, 7 and 9 are electron microscope images of aluminum alloy die castings without precipitation hardening treatment. Figure 2 , 4 , 6, 8 and 10 are electron microscope images of aluminum alloy die castings after precipitation hardening treatment.

[0023] Fig.11A The aluminum alloy elevated floor of Example 2 of the present disclosure; Fig. 11B The aluminum alloy elevated floor of Example 2 of the present disclosure is shown from another perspective.

[0024] Fig.12 This is the aluminum alloy elevated floor of Example 3 of the present disclosure.

[0025] Main component symbols

[0026] 1,2 Aluminum alloy raised floor

[0027] 10 top boards

[0028] 11. Border

[0029] 12 Rib structure

[0030] 20 Through holes. DETAILED DESCRIPTION

[0031] The following describes the implementation of the present disclosure through specific implementation schemes, and those skilled in the art of the present disclosure can easily understand the spirit, advantages and effects of the present disclosure based on the contents described herein. However, the implementation schemes described herein are not intended to limit the present disclosure, and the present disclosure can also be implemented or applied through other different implementation schemes, and the details described herein can also be given different changes or modifications according to different viewpoints and applications without departing from the spirit of the present disclosure.

[0032] The proportions, structures, sizes and other features shown in the drawings attached hereto are only used to match the contents described hereto so that those skilled in the art can read and understand the present disclosure, and are not used to limit the scope of implementation of the present disclosure. Therefore, any changes in the proportions, modifications in the structures, or adjustments in the sizes, without affecting the purposes and effects that can be achieved by the present disclosure, should fall within the scope that can be covered by the technical contents described hereto.

[0033] When it is described in this document that “includes,” “comprising,” or “has” specific elements, unless otherwise stated, other elements, components, structures, regions, parts, devices, systems, steps, or connections may also be included, rather than excluding such other elements.

[0034] Unless clearly stated otherwise herein, the singular forms "a", "an" and "the" described herein also include plural forms, and "or" and "and / or" described herein are used interchangeably.

[0035] The terms "upper" and "lower" described herein are only used to illustrate the implementation scheme of the present disclosure, and are not used to limit the scope of the present disclosure. The adjustment, interchange and change of their relative positions and relationships should be regarded as the scope of the present disclosure without substantially changing the technical content of the present disclosure.

[0036] Any numerical value within the numerical range described herein is included herein, and the numerical range described herein is inclusive and combinable, and any numerical value falling within the numerical range described herein can be used as the maximum or minimum value to derive a sub-range. For example, the numerical range of "3 to 9 wt % of magnesium" means that the numerical values ​​of 3 wt %, 3.5 wt %, 4 wt %, 4.5 wt %, 5 wt %, 5.5 wt %, 6 wt %, 6.5 wt %, 7 wt %, 7.5 wt %, 8 wt %, 8.5 wt %, 9 wt % within the range are included in the range referred to herein, and such numerical values ​​can derive sub-ranges, for example, 3.5 wt % to 9 wt %, 3 wt % to 8.5 wt %, 3.5 wt % to 8.5 wt %, etc.

[0037] The aluminum alloy elevated floor disclosed in the present invention comprises an aluminum alloy die-casting part, which can be formed by a general die-casting process or a vacuum die-casting process.

[0038] The aluminum alloy elevated floor including the aluminum alloy die casting can be in various shapes, such as triangle, rectangle, pentagon, hexagon, etc. The aluminum alloy elevated floors of various shapes can be placed / embedded in a frame matching it, and the frame is supported by a support frame so that there is a specific distance between the frame and the actual ground, and the specific distance can be controlled by the support frame. Each corner of the frame is a support point, one end of the support frame is connected to the support point, and the other end is connected to the actual ground, and the support frame is perpendicular to the actual ground and the aluminum alloy elevated floor, so as to achieve stable support. In one embodiment, the aluminum alloy elevated floor is rectangular and is placed / embedded in a rectangular frame. In another embodiment, the aluminum alloy elevated floor and the frame are both square.

[0039] In one embodiment, the aluminum alloy elevated floor is formed with through holes, and there may be multiple through holes, so that air can circulate and promote air cleanliness. In one embodiment, the aluminum alloy elevated floor is formed with multiple through holes, and the number, aperture and arrangement of the through holes affect the ventilation rate, and the present disclosure can obtain an aluminum alloy elevated floor with a ventilation rate of 17% to 50%. In one embodiment, the aluminum alloy elevated floor of the present disclosure is a honeycomb plate, such as a honeycomb plate with a ventilation rate of 17%, a honeycomb plate with a ventilation rate of 25%; in one embodiment, the aluminum alloy elevated floor of the present disclosure is a grille plate, such as a grille plate with a ventilation rate of 50%. The aluminum alloy elevated floor may also not be formed with holes, and is a blind plate, which can be used in places without ventilation requirements. On the other hand, in response to the need for visualization under the floor, the size of the through hole can be increased, and the remaining aluminum alloy elevated floor portion is used as a structure similar to a window frame, and a transparent window sheet is placed on the through hole or embedded in the through hole, so that the aluminum alloy elevated floor becomes a window floor.

[0040] In one embodiment, the aluminum alloy elevated floor of the present disclosure may be surface treated to enhance rust resistance, friction resistance, scratch resistance, corrosion resistance, acid and alkali corrosion resistance, and anti-slip properties. In one embodiment, the surface of the aluminum alloy die casting is surface treated to form at least one surface treatment layer selected from the group consisting of epoxy resin coating, nickel-chromium coating, powder coating, and anodizing.

[0041] In the present disclosure, the aluminum alloy elevated floor includes an aluminum alloy die-casting having a specific chemical element composition, which can improve the yield strength and load-bearing capacity, thereby facilitating the application of the aluminum alloy elevated floor. Specifically, the aluminum alloy die-casting includes: 7 to 11 weight % silicon, 3 to 9 weight % magnesium, 1 to 3 weight % copper, and the balance aluminum, wherein the aluminum alloy die-casting also has a magnesium silicide (Mg2Si) phase.

[0042] The aluminum alloy die casting includes 7 to 11 wt % silicon, such as, but not limited to, 7 wt %, 7.5 wt %, 8 wt %, 8.26 wt %, 8.35 wt %, 8.5 wt %, 8.53 wt %, 9 wt %, 9.5 wt %, 9.35 wt %, 9.65 wt %, 9.68 wt %, 10 wt %, 10.25 wt %, 10.26 wt %, 10.28 wt %, 10.5 wt %, or 11 wt %, etc. In other embodiments, the aluminum alloy die casting may include 7.5 to 10.5 wt % silicon, 7.5 to 9.5 wt % silicon, or 7.5 to 9 wt % silicon.

[0043] The aluminum alloy die casting includes 3 to 9 wt % magnesium, such as, but not limited to, 3 wt %, 3.11 wt %, 3.5 wt %, 3.6 wt %, 4 wt %, 4.5 wt %, 5 wt %, 5.17 wt %, 5.5 wt %, 5.73 wt %, 6 wt %, 6.5 wt %, 7 wt %, 7.5 wt %, 8 wt %, 8.5 wt %, or 9 wt %, etc. In other embodiments, the aluminum alloy die casting may include 3 to 8 wt % magnesium, 3 to 7 wt % magnesium, 3.5 to 6.5 wt % magnesium, 4 to 6.5 wt % magnesium, or 4 to 6 wt % magnesium.

[0044] The aluminum alloy die casting includes 1 to 3 wt % copper, such as, but not limited to, 1 wt %, 1.25 wt %, 1.5 wt %, 1.75 wt %, 1.85 wt %, 1.86 wt %, 2 wt %, 2.01 wt %, 2.25 wt %, 2.26 wt %, 2.29 wt %, 2.43 wt %, 2.4 wt %, 2.44 wt %, 2.5 wt %, 2.55 wt %, 2.75 wt %, 2.98 wt %, or 3 wt %, etc. In other embodiments, the aluminum alloy die casting may include 1 to 2.75 wt % copper, 1.25 to 2.75 wt % copper, 1 to 2.5 wt % copper, or 1.5 to 2.5 wt % copper.

[0045] Among the various elements of aluminum alloy die castings, silicon can be mainly used to improve fluidity, improve the thermal expansion, wear resistance and corrosion resistance of castings, etc. However, crystallized silicon easily forms hard spots, which makes the machinability worse. When the silicon content is low (such as 0.7%), the ductility of the aluminum alloy is good; when the silicon content is high (such as 7%), the ductility becomes lower. In the present disclosure, silicon is added to the aluminum alloy to improve the tensile strength and yield strength of the aluminum alloy. Magnesium can make the weldability of the aluminum alloy good and also provide the aluminum alloy with excellent corrosion resistance, but the ductility of the aluminum alloy containing magnesium is significantly worse, the solidification shrinkage ratio is large, and it is easy to have hot brittleness. When there are silicon and magnesium in the aluminum alloy, Mg2Si phase can be precipitated, which can improve the yield strength and tensile strength of the aluminum alloy, but on the other hand, the ductility is worse on the contrary. Therefore, the requirements of various properties must be considered to adjust the elemental composition of the aluminum alloy.

[0046] Copper in aluminum alloy can be used to enhance the strength and machinability of castings, especially it gives aluminum alloys a better solid solution strengthening effect. For example, CuAl2 precipitated by aging can bring obvious strengthening effect to aluminum alloys; however, copper will reduce the corrosion resistance of aluminum alloys. In the present disclosure, the aluminum alloy contains a small amount of copper to enhance the strength and facilitate further improving the strength of the casting when a solid solution strengthening process is required.

[0047] To achieve the above elemental composition, suitable amounts of various elements may be added to the aluminum liquid. In one embodiment, the aluminum liquid is ADC12, and the aluminum alloy die casting of modified ADC12 is obtained by adding suitable amounts of various elements, such as but not limited to adding pure magnesium blocks to the ADC12 aluminum liquid. In another embodiment, ADC5 and ADC14 may also be blended to obtain an aluminum alloy die casting having the above elemental composition.

[0048] The aluminum alloy die casting disclosed herein has a density of 2.6 g / cm 3 Above, 2.65g / cm 3 Above, or 2.7g / cm 3 Above, for example but not limited to 2.6 g / cm3 , 2.62g / cm 3 , 2.63g / cm 3 , 2.65g / cm 3 , 2.67g / cm 3 , 2.68g / cm 3 , 2.7g / cm 3 , 2.71g / cm 3 , 2.72g / cm 3 , 2.73g / cm 3 or 2.74 g / cm 3 Moreover, the aluminum alloy die casting of the present disclosure has a low porosity, which may be less than 10%, less than 8%, or less than 5%, such as but not limited to 10%, 9%, 8%, 7%, 6%, 5%, 4%, or 3%. The porosity can be controlled by various conditions and parameters in the die casting process, such as, for example, aluminum liquid temperature, mold temperature, degassing device improvement, or filling speed.

[0049] The aluminum alloy die casting disclosed herein has a yield strength of 200 MPa or more, 205 MPa or more, or 230 MPa or more, such as but not limited to 200 MPa, 205 MPa, 209 MPa, 210 MPa, 215 MPa, 220 MPa, 225 MPa, 230 MPa, or 233 MPa. The yield strength here is the data obtained without precipitation hardening treatment. If the aluminum alloy die casting is further subjected to precipitation hardening treatment, the yield strength can be further improved, such as 230 MPa or more, 240 MPa or more, or 250 MPa or more.

[0050] The aluminum alloy die casting disclosed herein has a tensile strength of 180 MPa or more, 190 MPa or more, or 200 MPa or more, such as but not limited to 180 MPa, 185 MPa, 188 MPa, 190 MPa, 191 MPa, 192 MPa, or 209 MPa. The aluminum alloy die casting disclosed herein has a Brinell hardness of 135 HB or more, or 140 HB or more, such as but not limited to 135 HB, 136 HB, 137 HB, 138 HB, 138.1 HB, 139 HB, 140 HB, 141 HB, 142 HB, 143 HB, 144 HB, or 144.6 HB.

[0051] The precipitation hardening treatment includes solution treatment, quenching treatment and aging treatment. Solution treatment is a heat treatment procedure in which the aluminum alloy is heated to a high-temperature single-phase region and then maintained at this temperature for a period of time to allow the excess phase to fully dissolve into the solid solution to obtain a supersaturated solid solution. Quenching treatment is a rapid cooling of the aluminum liquid, which generally enhances the strength and hardness of the aluminum alloy. Its influencing factors include the rate of rapid cooling. Aging treatment refers to a heat treatment procedure in which the aluminum alloy is placed for a period of time after undergoing solution treatment, cold plastic deformation, casting, forging and other procedures, and its performance, shape and size change over time. It is divided into artificial aging and natural aging. The difference is that artificial aging is placed in a specific temperature environment while natural aging is placed in a room temperature environment.

[0052] In the present disclosure, the aluminum alloy die casting may be subjected to precipitation hardening treatment, which includes a solution treatment procedure in which the aluminum alloy die casting is heated to 450°C to 550°C and maintained at the temperature for 1.5 to 2 hours, such as 500°C for 2 hours, 450°C for 1.5 hours, or 450°C for 2 hours; and an aging treatment for 1 to 24 hours for the aluminum alloy die casting after solution treatment and quenching treatment, such as natural aging or artificial aging. When artificial aging is used, the temperature may be 400°C to 600°C, such as 500°C for 120 minutes.

[0053] The present disclosure will be described in further detail with reference to the following examples, which are however in no way intended to limit the scope of the present disclosure.

[0054] Example 1

[0055] As shown in Table 1 below, 0.5 wt%, 1 wt%, 3 wt%, and 5 wt% of pure magnesium blocks were added to the solution formed by melting JIS standard ADC12. The magnesium blocks were stirred continuously while melting to be fully mixed, and then aluminum alloy die castings were made. The contents of magnesium, silicon, and copper in the obtained aluminum alloy die castings are listed in Table 2, and the aluminum alloy die castings were subjected to the following metallographic and density tests. In addition to stipulating the contents of magnesium, silicon, and copper, JIS standard ADC12 also limits the upper limits of the contents of elements such as titanium, manganese, iron, nickel, zinc, lead, and tin, but these elements are only present in trace amounts, so they are not discussed in this disclosure and the embodiments.

[0056] Table 1 Sample preparation

[0057] Sample No. ADC12 (wt%) Magnesium block (wt%) S0 100 0 S1 99.5 0.5 S2 99 1 S3 97 3 S4 95 5

[0058] Table 2 Contents of magnesium, silicon and copper in aluminum alloy die castings

[0059]

[0060] Metallographic structure test

[0061] Samples were taken from the aluminum alloy die castings of the embodiment, and were subjected to rough grinding, fine grinding, polishing, corrosion and other steps in sequence, and the metallographic structure of the aluminum alloy die castings was observed using a scanning electron microscope. Figure 1 , 3 , 5, 7 and 9 are electron microscope images of S0, S1, S2, S3 and S4 aluminum alloy die castings respectively. Figure 2 , 4 , 6, 8 and 10 are electron microscope images of S0, S1, S2, S3 and S4 aluminum alloy die castings after further precipitation hardening treatment, wherein the precipitation hardening treatment is a solution treatment at 500°C for 2 hours, a quenching treatment and a natural aging treatment for 24 hours.

[0062] Figure 1 , 3 , 5, 7 and 9 show that the S1, S2, S3 and S4 aluminum alloy die castings have α aluminum precipitation (white part) and aluminum eutectic phase (dark part). Figure 2 , 4 By comparing S1, S2, S3 and S4 aluminum alloy die castings, it can be found that the magnesium element or silicon element has been dissolved into the α-aluminum and refined grains are obtained.

[0063] Density test

[0064] The aluminum alloy die castings without precipitation hardening treatment were prepared into 4 mm and 6 mm thick test pieces suitable for universal testing machines, 3 pieces each. The total length of the test piece was 200 mm, the dimensions of the two shoulders were 51 mm long and 20 mm wide, and the dimensions of the central part were 80 mm long and 13.5 mm wide. The density of each test piece was tested with an electronic precision balance (model: Precisa ES 2220M, Quanhua Precision Co., Ltd.), and the average value was taken. The results are shown in Table 3 below.

[0065] Table 3 - Density

[0066]

[0067] Mechanical properties test

[0068] The aluminum alloy die castings that have been subjected to precipitation hardening treatment were prepared into test pieces with thicknesses of 4 mm and 6 mm suitable for a universal testing machine, 3 pieces each. The test piece size is the same as the test piece for the density test. The tensile strength of the aluminum alloy die castings was tested by clamping both ends of the test piece with a universal testing machine (model: HT-9102, Hongda Instrument Co., Ltd.), and the average value was taken. The results are shown in Table 4 below.

[0069] Table 4 - Tensile Strength

[0070]

[0071] According to the results in Table 4, ADC12 without additional magnesium block has higher tensile strength, and as the magnesium content in the aluminum alloy die casting increases, the tensile strength decreases.

[0072] The aluminum alloy die castings without precipitation hardening treatment were prepared into 4 mm and 6 mm thick test pieces suitable for universal testing machine, 3 pieces each. The test piece size was the same as the test piece for density test. The yield strength of the aluminum alloy die castings was tested by clamping the two ends of the test piece with the universal testing machine, and the average value was taken. The results are shown in Table 5 below.

[0073] Table 5 - Yield Strength

[0074]

[0075] According to the results in Table 5, ADC12 without additional magnesium blocks has a lower yield strength, and as the magnesium content in the aluminum alloy die casting increases, the yield strength gradually increases. Therefore, when used as an elevated floor, it can have a better bearing capacity.

[0076] The aluminum alloy die castings without precipitation hardening treatment and precipitation hardening treatment were prepared into test pieces suitable for universal testing machine, with thickness of 4 mm and 6 mm, 3 pieces each. The test piece size was the same as the test piece of density test. The elongation of the aluminum alloy die casting was tested by clamping the two ends of the test piece with the universal testing machine, and the average value was taken. The results are shown in Table 6 below.

[0077] Table 6 - Elongation

[0078]

[0079] According to the results in Table 6, the yield strength of ADC12 without additional magnesium block has a higher elongation, and as the magnesium content in the aluminum alloy die casting increases, the elongation decreases.

[0080] The aluminum alloy die castings without precipitation hardening treatment were prepared into test pieces suitable for hardness test, with thickness of 4 mm and 6 mm, 3 pieces each. The test piece size is the same as the test piece of density test. The Brinell hardness (HB) of the aluminum alloy die castings was tested by a hardness tester (model: TAD-Q5E, Dachang Trading Co., Ltd.), and the average value was taken. The results are shown in Table 7 below, where standard test conditions were adopted.

[0081] Table 7-Brinell Hardness

[0082]

[0083] According to the results in Table 7, the yield strength of ADC12 without additional magnesium block has a higher hardness. After slightly increasing the magnesium content in the aluminum alloy die casting, the hardness suddenly decreases, and then gradually increases with the increase of magnesium content. When the magnesium content is added at 5wt%, the hardness of the aluminum alloy die casting can reach the level of ADC12.

[0084] From the above data, it can be inferred that in the case of a high silicon content, further adding magnesium can cause magnesium and silicon to precipitate Mg2Si strengthening phase during the solidification process of the aluminum alloy, which can improve the yield strength of the aluminum alloy die casting, but it will be accompanied by sacrificing some tensile strength. For the application of elevated floors, the importance of yield strength is greater than tensile strength. Therefore, adjusting the magnesium content in the aluminum alloy elevated floor within the specific range described in the present disclosure can effectively improve the bearing capacity of the aluminum alloy elevated floor. In addition, the aluminum alloy die casting that has been subjected to precipitation hardening treatment can reduce or eliminate segregation, which can further highlight the effect of the Mg2Si strengthening phase. As shown in Table 4, the influence of Mg2Si strengthening on the relative elongation becomes greater.

[0085] Example 2

[0086] A rectangular aluminum alloy die casting was prepared according to the content of Example 1, which contained 4.5 wt % to 5.5 wt % of magnesium. Fig.11A and Fig. 11B The aluminum alloy elevated floor 1 shown has a top plate 10 and a frame 11 and a rib structure 12 arranged below the top plate 10, which can be assembled with a square frame and a support frame to form an elevated floor structure. Tests have shown that the aluminum alloy elevated floor has excellent load-bearing capacity.

[0087] Example 3

[0088] A rectangular aluminum alloy die casting was prepared as described in Example 2. Fig.12 The aluminum alloy elevated floor 2 shown has a top plate 10 and a frame 11 and a rib structure 12 (not shown) arranged below the top plate 10. The difference between Example 3 and Example 2 is that the top plate 10 of the aluminum alloy elevated floor is further formed with a plurality of through holes 20, so that it is a honeycomb plate with a ventilation rate of 17%. The aluminum alloy elevated floor has excellent load-bearing capacity after testing.

[0089] Example 4

[0090] As described in Example 3, the diameter of the through holes 20 of the aluminum alloy elevated floor is enlarged and rectangular, so as to prepare a grid plate with a ventilation rate of 50%. The aluminum alloy elevated floor has excellent load-bearing capacity after testing.

[0091] Example 5

[0092] As described in Example 3, the size of the through hole 20 is large enough to allow the line of sight to easily penetrate to the bottom of the aluminum alloy elevated floor, and a transparent window sheet can be placed on the through hole 20 or embedded in the through hole 20 to close the through hole 20, so that the aluminum alloy elevated floor becomes a window floor. The aluminum alloy elevated floor has excellent load-bearing capacity after testing.

Claims

1. An aluminum alloy elevated floor, comprising an aluminum alloy die-casting, wherein the aluminum alloy die-casting comprises: 7 to 11 wt % silicon; 3 to 9% by weight of magnesium; 1 to 3 wt. % copper; and The balance of aluminum, Wherein, the aluminum alloy die casting has a magnesium silicide phase.

2. The aluminum alloy elevated floor according to claim 1, which is formed with through holes to serve as a honeycomb plate, a grille plate or a window floor.

3. The aluminum alloy elevated floor according to claim 1, wherein: The surface of the aluminum alloy die casting is subjected to surface treatment to form at least one surface treatment layer selected from the group consisting of epoxy resin coating, nickel-chromium plating coating, powder coating, and anodizing.

4. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die casting includes 7.5 to 9.5 weight percent silicon.

5. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die casting includes 3.5 to 6.5 weight percent magnesium.

6. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die casting includes 4 to 6 weight percent magnesium.

7. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die casting includes 1.5 to 2.5 weight percent copper.

8. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die-casting is a modified ADC12 aluminum alloy die-casting.

9. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die-casting is made by die-casting by mixing ADC5 and ADC14.

10. The aluminum alloy elevated floor according to claim 1, wherein: The density of the aluminum alloy die casting is greater than 2.

6.

11. The aluminum alloy elevated floor according to claim 1, wherein: The tensile strength of the aluminum alloy die casting is above 190 MPa.

12. The aluminum alloy elevated floor according to claim 1, wherein: The yield strength of the aluminum alloy die casting is above 200 MPa.

13. The aluminum alloy elevated floor according to claim 1, wherein: The aluminum alloy die casting is subjected to artificial aging treatment.

14. The aluminum alloy elevated floor according to claim 13, wherein: The artificial aging treatment is performed at 500° C. for 120 minutes.