Polyimide film surface high-binding-force copper metallization method

Through the steps of plasma roughening, alkali ring opening and silver salt activation, combined with the conventional acid sulfate electroplating copper process, the problem of insufficient bonding force of the copper plating on the surface of the polyimide film was solved, and high bonding force and thickness of copper were achieved. Coatings to meet the needs of flexible circuits and microelectronics and reduce production costs and environmental impact.

CN118726976AInactive Publication Date: 2024-10-01XIAMEN UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410760170.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the process of surface metallization of polyimide films, it is difficult to achieve high bonding force and thick copper plating with existing technology, and commonly used oxidant treatments have problems such as dynamic changes in concentration and thermal damage, resulting in insufficient bonding force of the coating and high production costs. .

Method used

Using steps such as plasma roughening, alkali ring opening and degreasing, silver salt activation and electroless copper plating, the surface is treated by a plasma etching machine, using an alkaline degreasing solution and silver salt activation solution, combined with conventional acidic sulfate Electroplating copper process to achieve high bonding strength and thickness of copper plating.

Benefits of technology

The formation of a high-adhesion copper plating layer on the surface of the polyimide film is achieved, ensuring excellent adhesion between the copper layer and PI, meeting application needs in the field of flexible circuits and microelectronics, and reducing production costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726976A_ABST
    Figure CN118726976A_ABST
Patent Text Reader

Abstract

The invention discloses a method for metallizing high-binding-force copper on the surface of a polyimide film, which comprises the following steps of: (1) plasma coarsening: placing the polyimide film in an inductive coupling plasma etching machine for etching treatment to obtain the etched polyimide film; (2) alkali ring opening and oil removal: the etched polyimide film is placed in oil removal liquid to be subjected to heat treatment in cooperation with an ultrasonic vibration mode, and the ring-opened polyimide film with the clean surface is obtained; (3) silver salt activation: the polyimide film is placed in a silver salt activation solution for impregnation, adsorption and activation, and an activated polyimide film is obtained; (4) electroless copper plating: carrying out electroless copper plating and electric conduction on the activated PI; and (5) electrocoppering and thickening: carrying out electrocoppering and thickening on the conductive PI. After the polyimide film is subjected to roughening, alkali treatment ring opening, oil removal, activation, chemical copper plating and electrocoppering thickening through the method, a compact, continuous and uniform copper plating layer with good binding force with the PI surface can be obtained, and the application requirements in the fields of flexible circuits and microelectronics are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer surface metallization, and in particular relates to a method for high-binding copper metallization on the surface of a polyimide film. Background Art

[0002] Polyimide (PI) is a type of polymer containing an imide ring (-CO-NR-CO-) on the main chain and is one of the organic polymer materials with the best comprehensive performance. PI has the advantages of strong heat resistance, low dielectric constant, high mechanical strength, good stability, and soft matrix. The metallization of the metal layer on the surface of PI can give it more functions and applications. For example, metallized polyimide can be used to manufacture various sensors and high-performance flexible circuit boards, and can be used as thermal interface materials, structural materials for spacecraft, thermal conductive materials, and electronic packaging materials.

[0003] PI surface metallization usually includes the following steps: degreasing, roughening, sensitization-activation-chemical copper plating or surface grafting conductivity, electroplating copper thickening. Common degreasing methods for PI include organic solvent degreasing, oxidant degreasing, alkali degreasing, etc., the purpose is to completely remove the oil stains on the PI surface. Organic solvent degreasing usually consists of acetone, ethanol, ethyl acetate, etc. The degreasing effect usually increases with the increase of solution temperature, while excessively high temperature accelerates the evaporation of organic solvents and endangers the health of operators. Alkali degreasing usually consists of sodium hydroxide, potassium hydroxide and surfactants, which can quickly remove saponified oil and mineral oil on the PI surface, and realize PI surface ring opening to improve hydrophilicity. Oxidants have both degreasing and roughening effects, and are usually composed of peroxides, potassium permanganate, chromic acid, etc. Oxidants can react with oil stains to achieve rapid degreasing, but the concentration of the oxidant changes continuously and needs to be controlled in real time, and the oxidation products may adhere to the PI surface and are difficult to remove. Chemical copper plating conductivity treatment often uses palladium, silver and other solutions for sensitization-activation. Palladium activation solution is expensive, and palladium activation solution needs to go through the stannous chloride sensitization step. Silver activation solution is cheaper and has higher chemical stability. In addition to sensitization-activation-chemical copper plating conductive treatment, conductive polymers such as polyaniline, polythiophene, polypyrrole, etc. can also be used for conductive treatment, but the stability of conductive polymers is poor and the conductivity is insufficient.

[0004] CN 101094563A discloses a method for direct metallization of polyimide surface. The PI surface is first etched with an acidic peroxide solution, then contacted with an acidic permanganate solution, and then the PI is activated in an acidic persulfate activation solution, and then the PI treated as above is contacted with an acidic treatment solution containing at least one thiophene derivative and at least one sulfonic acid or sulfonic acid derivative, in order to form a polymer conductive layer on the PI surface. Finally, the PI is metallized in an acidic electroplating metallization bath. The process uses an oxidant to chemically remove oil and roughen the PI surface, and makes the PI surface conductive by constructing a conductive polymer.

[0005] CN 101736329A discloses a polyimide film activation solution and a method for metallizing a polyimide film. The polyimide film activation solution contains metal ions, ammonia and a polyimide film wetting agent, the pH of the polyimide film activation solution is 9-14, and the molar ratio of metal ions to ammonia is 1:4-8. The polyimide film is in contact with the activation solution; the polyimide film in contact with the activation solution is subjected to heat treatment or reduction treatment to obtain a surface metallized polyimide film. This solution simplifies the production process, and only requires two steps of activation and reduction, but does not involve roughening and oil removal and ring opening steps. The thickness of the obtained polyimide surface metallized film is relatively thin, which increases the difficulty of electroplating metal thickening.

[0006] CN 106894226A discloses a method for plating a metallized silver film on the surface of a polyimide fiber. First, the polyimide fiber is roughened in a copper sulfate solution, and then the roughened polyimide fiber is impregnated with a mixed solution of silver nitrate, ammonia water, 15-35 g / L glucose and a catalyst hexamethylenetetramine, thereby forming a metallized silver polyimide fiber. This process only proposes a method for metallizing a silver film on the surface of a polyimide, and fails to ensure that the silver film coating reaches a certain thickness and still has good bonding strength. In addition, it does not involve steps and technical features such as roughening and oil removal and ring opening.

[0007] The bonding strength between PI and the coating mainly depends on the pretreatment steps. Pretreatment includes roughening, degreasing and activation. Common roughening methods for PI include chemical and physical methods, which aim to improve the hydrophilicity of the PI surface and increase the roughness of the PI surface, thereby increasing the bonding strength of the subsequent coating. Chemical methods include oxidant etching and surface grafting modification, etc. The advantage is that it can significantly improve the surface properties of PI, but during the oxidant etching process, the oxidant concentration changes dynamically and needs to be detected in real time. The oxidation products are easy to adhere to the PI surface and are difficult to remove; due to the small number of active sites on the PI molecular chain, the rate of grafting reaction is slow, resulting in low grafting efficiency, and the selectivity of the grafting reaction is also poor, which may introduce some unnecessary functional groups. Physical methods include laser etching, plasma etching, ultrasonic vibration, etc.: Laser etching can accurately control the etching area and depth to achieve high-precision surface roughening, but it may cause thermal damage to the PI substrate and has high cost; ultrasonic vibration equipment is simple, easy to operate, and low cost. It can achieve surface roughening without damaging the substrate, but the roughening effect is limited and it is difficult to fully meet the requirements of high bonding strength between the coating and PI. Plasma etching can form a high-density and uniform rough structure on the PI surface and can be performed at a lower temperature to avoid thermal damage.

[0008] Therefore, in view of the technical requirements of PI surface metallization characteristics, it is crucial to invent a simple, efficient, controllable, economical, high-bonding copper metallization technology for PI surface with good bonding between PI and thicker copper plating. Summary of the invention

[0009] The purpose of the present invention is to overcome the above-mentioned deficiencies in the prior art and provide a polyimide film surface high-binding copper metallization technology.

[0010] The technical solution of the present invention is as follows:

[0011] A method for high-binding copper metallization on the surface of a polyimide film, characterized in that it comprises the following steps:

[0012] (1) Plasma roughening: placing the polyimide film in an inductively coupled plasma etcher for etching to obtain an etched polyimide film;

[0013] (2) Alkali ring opening and degreasing: The etched polyimide film is placed in a degreasing solution and subjected to heat treatment in combination with ultrasonic vibration to obtain a clean and ring-opened polyimide film; the degreasing solution uses deionized water as a solvent and contains sodium phosphate, sodium hydroxide, sodium carbonate, sodium silicate and OP-10;

[0014] (3) silver salt activation: placing the clean and open-loop polyimide membrane in a silver salt activation solution for immersion adsorption activation to obtain an activated polyimide membrane; the silver salt activation solution uses deionized water as a solvent and contains a soluble silver salt, a complexing agent and L-ascorbic acid;

[0015] (4) Chemical copper plating: The activated polyimide film is subjected to chemical copper plating for conductivity;

[0016] (5) Electroplating copper thickening: The polyimide film that has been made conductive by chemical copper plating in step (4) is electroplated with copper to thicken it.

[0017] In a preferred embodiment of the present invention, in the degreasing liquid, the concentration of sodium phosphate is 10-100 g / L, the concentration of sodium hydroxide is 20-160 g / L, the concentration of sodium carbonate is 10-60 g / L, the concentration of sodium silicate is 10-60 g / L, and the concentration of OP-10 is 3-10 g / L.

[0018] In a preferred embodiment of the present invention, in the silver salt activation solution, the concentration of soluble silver salt is 0.1-3 g / L, the complexing agent is 0.1-3 g / L, and the L-ascorbic acid is 0.1-1 g / L.

[0019] Further preferably, the soluble silver salt is at least one of silver nitrate, silver acetate and silver chlorate.

[0020] More preferably, the complexing agent is at least one of ammonia water, sodium carboxymethyl cellulose, triethanolamine, ethylenediamine and ethanolamine.

[0021] In a preferred embodiment of the present invention, in the step (1), the etching power is 10 to 600 W and the etching time is 30 to 1200 s.

[0022] In a preferred embodiment of the present invention, in step (2), the heat treatment temperature is 40 to 80° C. and the time is 5 to 35 minutes.

[0023] In a preferred embodiment of the present invention, in step (3), the temperature of the impregnation adsorption activation is 15 to 45° C. and the time is 1 to 10 minutes.

[0024] In a preferred embodiment of the present invention, in the step (1), the etching power is 10 to 600 W and the time is 30 to 1200 s; in the step (2), the heat treatment temperature is 40 to 80° C. and the time is 5 to 35 min; in the step (3), the immersion adsorption activation temperature is 15 to 45° C. and the time is 1 to 10 min.

[0025] In a preferred embodiment of the present invention, in step (5), a conventional acid sulfate copper electroplating process is used with a current density of 2A / dm 2 The electroplating time is 5 to 40 minutes, and the electroplated copper is thickened to 2 to 15 μm.

[0026] The beneficial effects of the present invention are:

[0027] 1. The present invention uses plasma treatment, which has a simple and controllable operation method. Dense micropores are generated on the PI surface, and the catalytic silver particles on the PI surface are small and non-agglomerated after activation treatment, thereby ensuring excellent bonding between the copper plating layer and the PI.

[0028] 2. The alkaline treatment ring opening and degreasing liquid in the present invention uses green, environmentally friendly, water-soluble detergents and surfactants, and the preparation method is simple, low-cost and environmentally friendly. PI is degreased by alkaline degreasing liquid and combined with ultrasonic vibration cleaning, which not only effectively removes oil stains on the surface of PI, but also achieves ring opening and improves hydrophilicity.

[0029] 3. The present invention uses silver salt solution instead of activated palladium as the activation solution for chemical copper plating, which is more economical and has a stronger adsorption effect with the substrate, and the subsequent coating bonding is better.

[0030] 4. The present invention first performs plasma roughening, then performs alkaline treatment for ring opening and oil removal. If the conventional process route is followed to perform ring opening and oil removal and then plasma roughening, the PI with no oil on the surface after oil removal and ring opening is easily contaminated in the subsequent process, which increases the cleaning step, and the plasma treatment also etches the alkaline treatment ring opening structure on the PI surface, thereby reducing the adsorption of subsequent activated silver ions / particles, and further reducing the bonding force between the copper plating layer and the PI.

[0031] 5. The copper layer thickened by electroplating copper in the present invention adopts the conventional acid sulfate electroplating copper process, and the copper layer thickened by electroplating copper still has good bonding strength with PI. In contrast, the copper layer on the surface of PI is easy to fall off by using the alkaline electroplating copper process.

[0032] 6. After PI is roughened, opened by alkali treatment, degreased, activated, electroplated with copper for conductivity, and thickened by copper electroplating according to the method of the present invention, a dense, continuous and uniform electroless copper coating with good adhesion to the PI surface can be obtained, and the copper layer thickness is 0.1-1 μm; after further thickening by copper electroplating to 2-15 μm, the coating is squared with a grid knife, adhered with 3M tape and torn at 180°. According to the requirements of ASTM D3359, the copper coating adhesion reaches 5B standard, which can meet the application requirements of flexible circuits and microelectronics. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Surface SEM morphology photographs (magnified 5000 times) of the clean and open-ring PI (a), the activated PI and the conductive PI of Example 1 of the present invention.

[0034] Figure 2 These are photos of dynamic contact angles of the untreated PI surface, the PI surface treated with plasma roughening, and the PI surface treated with alkali ring opening and degreasing in Example 1 of the present invention.

[0035] Figure 3 The surface appearance photograph (a) of the electroplated copper thickened PI prepared in Example 1 of the present invention and the appearance photograph (b) after being scratched with a grid knife and torn with 3M tape.

[0036] Figure 4 This is a cross-sectional metallographic microscope photograph of the surface copper plating layer of the electroplated copper thickened PI obtained in Example 1 of the present invention.

[0037] Figure 5 Surface SEM morphology photographs (magnified 5000 times) of the clean and open-ring PI (a), the activated PI and the conductive PI of Example 2 of the present invention.

[0038] Figure 6 These are photos of dynamic contact angles of the untreated PI surface, the PI surface treated with plasma roughening, and the PI surface treated with alkali ring opening and degreasing in Example 2 of the present invention.

[0039] Figure 7 The surface appearance photograph (a) of the electroplated copper thickened PI prepared in Example 2 of the present invention and the appearance photograph (b) after being scratched with a grid knife and torn with 3M tape.

[0040] Figure 8 This is a cross-sectional metallographic microscope photograph of the surface copper plating layer of the electroplated copper thickened PI obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0042] Example 1

[0043] (1) 30 g of sodium phosphate, 50 g of sodium hydroxide, 20 g of sodium carbonate, 10 g of sodium silicate and an appropriate amount of deionized water were stirred and mixed uniformly, and then 8 g of OP-10 was added while stirring, and then the volume was adjusted to 1 L with deionized water, and then stirred and mixed uniformly to obtain an alkaline degreasing liquid;

[0044] (2) 0.8 g of sodium carboxymethyl cellulose and an appropriate amount of deionized water were stirred and mixed uniformly, and then 0.5 g of silver nitrate was added under continuous stirring, and 0.5 g of L-ascorbic acid was added in a constant temperature water bath at a temperature of 60° C., and then the volume was made up to 1 L with deionized water, and stirred and mixed uniformly to obtain a silver salt activation solution;

[0045] (3) Plasma roughening: PI (whose contact angle is Figure 2 a) was placed in an inductively coupled plasma etcher for etching at a power of 200 W for 500 s to obtain an etched PI with a dynamic contact angle of 85° (the contact angle is shown in FIG. Figure 2 b);

[0046] (4) Alkali ring opening and degreasing: The etched PI obtained in step (3) is placed in the alkaline degreasing solution obtained in step (1) and subjected to heat treatment in combination with ultrasonic vibration. The heat treatment temperature is 70° C. and the time is 15 min. A clean and ring-opened PI with a dynamic contact angle of 21° is obtained (e.g. Figure 2 c), its surface SEM morphology is as follows Figure 1 As shown in a;

[0047] (5) Silver salt activation: The clean and open-ring PI obtained in step (4) was placed in the above silver salt activation solution at a temperature of 25° C. for immersion adsorption activation for 5 min to obtain an activated PI, whose surface activated silver layer was dense and the silver particles were fine, with an average particle size of 0.5 μm (e.g. Figure 1 b);

[0048] (6) Chemical copper plating: The activated PI obtained in step (5) was placed in a chemical copper plating solution at a temperature of 40°C for 30 min (30 g / L CuSO 4 ·5H 2 O, 52g / L Na 2 EDTA·2H 2 O, 10mg / LK 4 Fe(CN) 6 , 10 mg / L 2,2'-bipyridine, 3 g / L formaldehyde), to obtain Figure 1 c conductive PI;

[0049] (7) Electroplating copper thickening: The conductive PI obtained in step (6) is electroplated with conventional acid sulfate copper plating process (200 g / L CuSO 4 ·5H 2 O, 50g / LH 2 SO 4 、50mg / L Cl - , 200mg / L PEG, 1mg / L SPS), current density 2A / dm 2 , electroplating time 24min, electroplated copper thickened to about 10μm (such as Figure 4 As shown), we get Figure 3 a's electroplated copper thickened PI.

[0050] (8) Adhesion test: Use a grid knife to draw squares on the surface of the coating, adhere with 3M tape and tear it at 180 degrees. The copper layer does not fall off (such as Figure 3 As shown in b), the copper plating adhesion reaches 5B standard as required by ASTM D3359.

[0051] Example 2

[0052] (1) 90 g of sodium phosphate, 90 g of sodium hydroxide, 60 g of sodium carbonate, 50 g of sodium silicate and an appropriate amount of deionized water were stirred and mixed uniformly, and then 10 g of OP-10 was added while stirring, and then the volume was adjusted to 1 L with deionized water, and then stirred and mixed uniformly to obtain a degreasing liquid;

[0053] (2) 0.8 g of sodium carboxymethyl cellulose and an appropriate amount of deionized water were stirred and mixed uniformly, and then 0.5 g of silver nitrate was added under continuous stirring, and 0.5 g of L-ascorbic acid was added in a constant temperature water bath at a temperature of 60° C., and then the volume was made up to 1 L with deionized water, and stirred and mixed uniformly to obtain a silver salt activation solution;

[0054] (3) Plasma roughening: PI (whose contact angle is Figure 6a) was placed in an inductively coupled plasma etcher for etching at a power of 400 W for 600 s to obtain an etched PI with a dynamic contact angle of 87° (as shown in FIG. Figure 6 b), its surface SEM morphology is as follows Figure 5 As shown in a;

[0055] (4) Alkali ring opening and degreasing: The etched PI obtained in step (3) is placed in the degreasing solution obtained in step (1) and subjected to heat treatment in combination with ultrasonic vibration. The heat treatment temperature is 70° C. and the time is 15 min. A clean and ring-opened PI with a dynamic contact angle of 21° is obtained (e.g. Figure 6 c);

[0056] (5) Silver salt activation: The clean and open-ring PI obtained in step (4) was placed in the above silver salt activation solution at a temperature of 35° C. for immersion adsorption activation for 5 min to obtain an activated PI, whose surface activated silver layer was dense and the silver particles were fine, with an average particle size of 0.25 μm (e.g. Figure 5 b);

[0057] (6) Chemical copper plating: The activated PI obtained in step (5) was placed in a chemical copper plating solution at a temperature of 40°C for 30 min (30 g / L CuSO 4 ·5H 2 O, 52g / L Na 2 EDTA·2H 2 O, 10mg / LK 4 Fe(CN) 6 , 10 mg / L 2,2'-bipyridine, 3 g / L formaldehyde), to obtain Figure 5 c conductive PI;

[0058] (7) Electroplating copper thickening: The conductive PI obtained in step (6) is electroplated with conventional acid sulfate copper plating process (200 g / L CuSO 4 ·5H 2 O, 50g / LH 2 SO 4 、50mg / L Cl - , 200mg / L PEG, 1mg / L SPS), current density 2A / dm 2 , electroplating time 24min, electroplated copper thickened to about 10μm (such as Figure 8 As shown), we get Figure 7 a's electroplated copper thickened PI.

[0059] (8) Adhesion test: Use a grid knife to draw squares on the surface of the coating, adhere with 3M tape and tear it at 180 degrees. The copper layer does not fall off (such as Figure 7As shown in b), the copper plating adhesion reaches 5B standard as required by ASTM D3359.

[0060] Comparative Examples 1 to 5

[0061] The process of Comparative Examples 1 to 5 refers to Examples 1 and 2, and the test methods are the same as those of Examples 1 and 2. The specific process conditions and test results are shown in Table 1 below:

[0062] Table 1

[0063]

[0064]

[0065] It can be found from the above Examples 1 to 2 and Comparative Examples 1 to 5 that increasing the concentration of sodium hydroxide in the degreasing solution can increase the bonding force between the copper plating layer and PI, which is attributed to increasing the degree of ring opening on the PI surface and increasing the adsorption of silver salt.

[0066] It can be found from the above Examples 1 to 2 and Comparative Examples 1 to 5 that silver salt activation instead of palladium salt activation can improve the bonding force between the copper plating layer and PI, which is attributed to the fact that the structure of the carboxylate generated by the ring opening of PI has a stronger adsorption capacity for silver ions.

[0067] It can be found from the above-mentioned Examples 1 to 2 and Comparative Examples 1 to 5 that as the plasma treatment power increases, the bonding force between the copper plating layer and the PI also increases. This is attributed to the increase in the density of pits on the PI surface after the plasma treatment, so that the catalytic silver layer on the PI surface after activation is denser and the particles are finer.

[0068] It can also be found from the above Examples 1 to 2 and Comparative Examples 1 to 5 that the order of pre-treatment steps will also affect the bonding strength between PI and the copper layer. The bonding effect is best in the order of roughening first, then alkaline treatment for ring opening and degreasing, and then activation. This is attributed to the fact that the ring opening occurs first on the PI surface, and then plasma treatment is performed. The plasma will etch away part of the ring-opening structure, thereby affecting the subsequent adsorption of activated particles.

[0069] In summary, by adopting the process of the present invention, a dense, continuous, uniform copper plating layer with good bonding strength with PI can be obtained.

[0070] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for high-binding copper metallization on the surface of a polyimide film, characterized in that: The steps include: (1) Plasma roughening: placing the polyimide film in an inductively coupled plasma etcher for etching to obtain an etched polyimide film; (2) Alkali ring opening and degreasing: The etched polyimide film is placed in a degreasing solution and subjected to heat treatment in combination with ultrasonic vibration to obtain a clean and ring-opened polyimide film; the degreasing solution uses deionized water as a solvent and contains sodium phosphate, sodium hydroxide, sodium carbonate, sodium silicate and OP-10; (3) silver salt activation: placing the clean and open-loop polyimide membrane in a silver salt activation solution for immersion adsorption activation to obtain an activated polyimide membrane; the silver salt activation solution uses deionized water as a solvent and contains a soluble silver salt, a complexing agent and L-ascorbic acid; (4) Chemical copper plating: The activated polyimide film is subjected to chemical copper plating for conductivity; (5) Electroplating copper thickening: The polyimide film made conductive by chemical copper plating in step (4) is electroplated copper thickening.

2. A method for high-bonding copper metallization on a polyimide film surface as claimed in claim 1, characterized in that: In the degreasing liquid, the concentration of sodium phosphate is 10-100 g / L, the concentration of sodium hydroxide is 20-160 g / L, the concentration of sodium carbonate is 10-60 g / L, the concentration of sodium silicate is 10-60 g / L, and the concentration of OP-10 is 3-10 g / L.

3. A method for high-bonding copper metallization on a polyimide film surface as claimed in claim 1, characterized in that: In the silver salt activation solution, the concentration of soluble silver salt is 0.1-3 g / L, the concentration of complexing agent is 0.1-3 g / L, and the concentration of L-ascorbic acid is 0.1-1 g / L.

4. A method for high-bonding copper metallization on a polyimide film surface as claimed in claim 3, characterized in that: The soluble silver salt is at least one of silver nitrate, silver acetate and silver chlorate.

5. A method for high-bonding copper metallization on a polyimide film surface as claimed in claim 3, characterized in that: The complexing agent is at least one of ammonia water, sodium carboxymethyl cellulose, triethanolamine, ethylenediamine and ethanolamine.

6. A method for high-bonding copper metallization on the surface of a polyimide film according to any one of claims 1 to 5, characterized in that: In the step (1), the etching power is 10 to 600 W and the etching time is 30 to 1200 s.

7. A method for high-bonding copper metallization on a polyimide film surface as claimed in any one of claims 1 to 5, characterized in that: In the step (2), the heat treatment temperature is 40 to 80° C. and the time is 5 to 35 minutes.

8. A method for high-bonding copper metallization on the surface of a polyimide film according to any one of claims 1 to 5, characterized in that: In the step (3), the temperature for the immersion adsorption activation is 15 to 45° C. and the time is 1 to 10 minutes.

9. A method for high-bonding copper metallization on the surface of a polyimide film according to any one of claims 1 to 5, characterized in that: In the step (1), the etching power is 10 to 600 W and the time is 30 to 1200 s; in the step (2), the heat treatment temperature is 40 to 80° C. and the time is 5 to 35 min; in the step (3), the immersion adsorption activation temperature is 15 to 45° C. and the time is 1 to 10 min.

10. A method for high-bonding copper metallization on the surface of a polyimide film according to any one of claims 1 to 5, characterized in that: In the step (5), a conventional acid sulfate copper electroplating process is used with a current density of 2A / dm 2 The electroplating time is 5 to 40 minutes, and the electroplated copper is thickened to 2 to 15 μm.

Citation Information

Patent Citations

  • Preparation method of polyimide non-adhesive flexible printed circuit board

    CN106413266A

  • Polyimide pipe film surface metallization electroplating method

    CN115928166A

  • Method of manufacturing flexible printed board

    JP2004079660A

  • Method for preparation of polyimide surface for chemical metal coating

    RU2607627C1

  • Method of fabricating flexible film

    US20100183824A1