Negative electrode for hydrogen production by alkaline electrolysis of water

By using porous carbon/carbon composite materials as the cathode electrode matrix for alkaline electrolysis of water to produce hydrogen, and loading water electrolysis catalysts, the problems of insufficient catalytic activity and corrosion resistance of cathode materials in the existing technology are solved, and efficient and stable hydrogen production is achieved. Generation and long life electrodes.

CN118727033AActive Publication Date: 2024-10-01XIAN CHAOMA SCI TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411008588.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-01
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing cathode electrode materials in alkaline water electrolysis for hydrogen production have problems such as poor catalytic activity, poor resistance to strong alkali corrosion, short life under high current density, and weak catalyst coating bonding, which affects the hydrogen production efficiency and the service life of the electrolyzer.

Method used

Porous carbon/carbon composite material is used as the cathode electrode matrix, and the specific surface area and conductivity are increased through graphitization treatment, and a water electrolysis catalyst is loaded to form a cathode electrode with high hydrogen evolution catalytic activity and durability.

Benefits of technology

The hydrogen evolution catalytic activity and service life of the cathode are improved, the hydrogen production energy consumption is reduced, the process is simple, the cost is low, and it is suitable for large-scale application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727033A_ABST
    Figure CN118727033A_ABST
Patent Text Reader

Abstract

The invention relates to a negative electrode for hydrogen production by alkaline electrolysis of water, and belongs to the technical field of hydrogen production by alkaline electrolysis of water. The negative electrode is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst loaded on the porous carbon / carbon composite material matrix; the graphitization degree of the porous carbon / carbon composite material matrix is 90-99%, the specific surface area is 0.7-2.5 m < 2 > / g, the contact angle is 110-160 degrees, and the compressive strength is not less than 1.6 MPa. The negative electrode is stable in structure, resistant to strong alkali corrosion, capable of stably running for a long time, small in density, high in water electrolysis catalyst loading capacity, high in hydrogen production efficiency, beneficial to reduction of hydrogen production energy consumption, simple in preparation process, easy to operate and low in cost, and has good application prospects in the aspect of hydrogen production through alkaline electrolysis of water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] The invention relates to a cathode electrode used for producing hydrogen by alkaline water electrolysis, belonging to the technical field of producing hydrogen by alkaline water electrolysis. Background Art

[0004] Hydrogen energy is a green, low-carbon, high-calorific value, renewable green energy with diverse storage and transportation methods and a wide range of application scenarios. It is regarded as the ultimate energy under the "dual carbon" goal. Green hydrogen is generated by using renewable clean energy such as light energy and wind energy to generate hydrogen through the electrolysis of water, truly achieving the "decarbonization" of energy.

[0005] Alkaline solution water electrolysis (ALK) is the largest and most commercially applied technology in the green hydrogen production route to date. The electrolyzer is the key equipment for hydrogen production by alkaline solution water electrolysis. The quality of the core component, the cathode electrode, directly determines the efficiency and capacity of hydrogen production. The commercial cathode electrode is based on a nickel mesh and sprayed with Raney nickel powder to prepare the electrode material. This electrode material has poor catalytic activity, poor resistance to strong alkali corrosion, short life at high current density, weak bonding with the catalyst coating and easy peeling, etc., which directly affects the service life of the electrolyzer and the efficiency of hydrogen production. Summary of the invention

[0007] In view of the shortcomings of cathode electrode materials in the current alkaline water electrolysis hydrogen production, the present invention provides a cathode electrode for alkaline water electrolysis hydrogen production. The cathode electrode uses a porous carbon / carbon composite material as a matrix. The porous structure of the matrix can not only provide a channel for alkali solution and charge transfer in the process of water electrolysis hydrogen production, but also make it have a larger specific surface area, which is beneficial to increase the effective load of water electrolysis catalyst and improve the combination effect with the water electrolysis catalyst. Compared with metal matrix materials, the matrix also has the characteristics of low density and strong alkali corrosion resistance. The cathode electrode made by loading the water electrolysis catalyst on the matrix has high hydrogen evolution catalytic activity and can operate stably for a long time, and has good application prospects in alkaline water electrolysis hydrogen production.

[0008] The objectives of the present invention are achieved through the following technical solutions.

[0009] A cathode electrode for producing hydrogen by alkaline water electrolysis, the cathode electrode being composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the porous carbon / carbon composite material matrix;

[0010] The graphitization degree of the porous carbon / carbon composite material matrix is ​​90-99%, and the specific surface area is 0.7-2.5m 2 / g, contact angle is 110~160 o , compressive strength is not less than 1.6MPa.

[0011] Preferably, the porous carbon / carbon composite material substrate is subjected to roughening pretreatment before loading the water electrolysis catalyst. The roughening pretreatment can further increase the specific surface area of ​​the porous carbon / carbon composite material substrate and reduce the contact angle of the porous carbon / carbon composite material substrate, thereby improving the loading effect of the water electrolysis catalyst on the porous carbon / carbon composite material substrate. More preferably, the specific surface area of ​​the porous carbon / carbon composite material substrate after roughening pretreatment is 1~4m 2 / g, contact angle is 60~110 o .

[0012] Preferably, the porous carbon / carbon composite material matrix is ​​roughened by gas phase oxidation, liquid phase oxidation or a combination of the two. More preferably, the gas phase oxidation method is to place the porous carbon / carbon composite material matrix at 350-600 o C for 15 to 50 minutes. The liquid phase oxidation method is to place the porous carbon / carbon composite material matrix in a 5 to 30 wt.% acid solution for oxidation for 10 to 30 minutes.

[0013] Preferably, the porous carbon / carbon composite material matrix is ​​formed by graphitizing a porous skeleton carbon and a second phase carbon covering the surface of the porous skeleton carbon; more preferably, the density of the porous skeleton carbon is 0.05-0.7 g / cm 3 The density of the porous skeleton carbon covered with the second phase carbon is 0.14~1g / cm 3 .

[0014] Preferably, the porosity of the porous skeleton carbon is 35-80%; more preferably, the pore size of the porous skeleton carbon is 50-500 μm.

[0015] Preferably, after the second phase carbon is covered on the porous skeleton carbon, o C for 1 to 6 hours to form the porous carbon / carbon composite material matrix.

[0016] Preferably, the porous skeleton carbon is prepared using carbon fiber braid or foam carbon as a precursor.

[0017] Preferably, the porous skeleton carbon prepared from carbon fiber braid has a pore size of 100-500 μm and a porosity of 35-60%; the porous skeleton carbon prepared from foamed carbon has a pore size of 50-300 μm and a porosity of 40-80%.

[0018] Preferably, the second phase carbon is formed by depositing a carbon source gas on the porous skeleton carbon through a chemical vapor deposition process; more preferably, the carbon source gas includes but is not limited to natural gas, propylene or acetylene, and the deposition temperature of the chemical vapor deposition process is 800-1100 oC, carbon source gas flow rate is 1~5m 3 / h, the deposition time is 50~100h;

[0019] Alternatively, the second phase carbon is formed by cracking a carbon source liquid on the porous skeleton carbon through a liquid phase impregnation process; more preferably, the carbon source liquid includes but is not limited to asphalt, phenolic resin or epoxy resin, and the cracking temperature of the liquid phase impregnation process is 900-1000 o C, lysis time is 1~5h;

[0020] Alternatively, a portion of the second phase carbon is formed by deposition of the carbon source gas on the porous framework carbon through a chemical vapor deposition process, and another portion is formed by cracking of the carbon source liquid on the porous framework carbon through a liquid phase impregnation process.

[0021] Preferably, the porous skeleton carbon prepared from the carbon fiber braid has a density of 0.6-0.7 g / cm 3 The density of the second phase carbon covered on the porous skeleton carbon is 0.8~1g / cm 3 ; Porous skeleton carbon prepared from foamed carbon, the density of porous skeleton carbon is 0.05~0.12g / cm 3 The density of the porous skeleton carbon covered with the second phase carbon is 0.14~0.25g / cm 3 .

[0022] Preferably, the porous skeleton carbon prepared from the carbon fiber braid has a graphitization degree of 96-99%, a resistivity of 1-10 mΩ·cm, and a specific surface area of ​​1-2.5 m 2 / g, contact angle is 110~150 o The porous skeleton carbon prepared based on foamed carbon has a graphitization degree of 90-97%, a resistivity of 10-20 mΩ·cm, and a specific surface area of ​​0.7-1 m 2 / g, contact angle is 130~160 o .

[0023] Preferably, the porous carbon / carbon composite material matrix prepared from the porous skeleton carbon prepared from the carbon fiber braid has a specific surface area of ​​2 to 4 m 2 / g, contact angle is 60~90 o The porous carbon / carbon composite material matrix prepared by porous skeleton carbon prepared by foam carbon has a specific surface area of ​​1~2m after roughening pretreatment. 2 / g, contact angle is 70~110 o .

[0024] Preferably, the water electrolysis catalyst is at least one of an alloy of a transition metal, an oxide of a transition metal, and a carbide of a transition metal. More preferably, the alloy of the transition metal is a nickel-iron alloy, and the molar ratio of nickel to iron is further preferably 7:1 to 1:1; the oxide of the transition metal is a nickel-zinc oxide, and the molar ratio of nickel to zinc is further preferably 7:3 to 1:1; the carbide of the transition metal is nickel carbide; when the alloy of the transition metal, the oxide of the transition metal, and the carbide of the transition metal are used in combination, it is further preferred to be a composite of a nickel-iron alloy and nickel carbide, and the molar ratio of the nickel-iron alloy to the nickel carbide is further preferably 1:(1 to 3).

[0025] Preferably, the particle size of the water electrolysis catalyst supported on the porous carbon / carbon composite material matrix is ​​0.005-2 μm (ie, 5 nm-2 μm).

[0026] Preferably, the thickness of the water electrolysis catalyst supported on the porous carbon / carbon composite material substrate is 0.03-5 μm (ie, 30 nm-5 μm).

[0027] Preferably, the water electrolysis catalyst is loaded on the porous carbon / carbon composite material matrix by the following method:

[0028] Hydrothermal method: dissolving the transition metal salt and alkaline substance in water, then transferring them to a reactor and adding a porous carbon / carbon composite material matrix to form transition metal oxides on the porous carbon / carbon composite material matrix through a hydrothermal reaction;

[0029] Electrodeposition method: using transition metal salts to prepare electrolyte solutions, using constant potential deposition method to form transition metal alloys on a porous carbon / carbon composite material matrix as a cathode;

[0030] Vapor deposition method: using vapor deposition process (physical vapor deposition process or / and chemical vapor deposition process) to deposit transition metal carbides on a porous carbon / carbon composite material matrix;

[0031] Electrodeposition + vapor deposition: first, an alloy of transition metals is formed on a porous carbon / carbon composite material matrix by electrodeposition, and then a carbide of transition metals is formed on the porous carbon / carbon composite material matrix by vapor deposition, that is, a composite catalyst of transition metal alloys and transition metal carbides is formed on the porous carbon / carbon composite material matrix.

[0032] Preferably, the specific surface area of ​​the cathode electrode is 1.1-4.2 m 2 / g, density is 0.5~1.8g / cm 3 .

[0033] Beneficial effects:

[0034] (1) The cathode electrode of the present invention adopts a porous carbon / carbon composite material as a loading matrix for loading a water electrolysis catalyst. On the one hand, the presence of its porous structure can provide a channel for alkali solution and charge transfer. On the other hand, compared with a metal matrix, the porous carbon / carbon composite material matrix has a smaller density, a higher specific surface area, and excellent resistance to strong alkali corrosion, which is beneficial to increase the effective loading of the water electrolysis catalyst. It also has a better bonding effect with the water electrolysis catalyst, making the cathode electrode structure stable, ensuring the cathode electrode's excellent hydrogen evolution catalytic activity and long-term stable operation.

[0035] (2) The present invention performs a roughening pretreatment on the porous carbon / carbon composite material matrix, which can further increase its surface area on the one hand, and further improve its bonding effect with the water electrolysis catalyst on the other hand, which is beneficial to further improve the hydrogen evolution catalytic activity and service life of the cathode electrode.

[0036] (3) The porous carbon / carbon composite material matrix described in the present invention is formed by graphitizing porous skeleton carbon and second phase carbon covering the surface of the porous skeleton carbon. The porous skeleton carbon as the matrix and the second phase carbon as the reinforcing phase are used in combination to achieve a higher degree of graphitization, so that the carbon atoms in the porous carbon / carbon composite material matrix are arranged in a more orderly manner, thereby improving the electrical conductivity of the porous carbon / carbon composite material matrix, meeting the electrical conductivity and strength requirements of the cathode in alkaline water electrolysis hydrogen production for the substrate loaded with water electrolysis catalyst. In addition, the substrate has a relatively small density, a relatively high specific surface area, and excellent resistance to strong alkali corrosion, which lays a foundation for the subsequent excellent hydrogen evolution catalytic performance of the cathode.

[0037] (4) In the cathode electrode described in the present invention, the porous carbon / carbon composite material matrix is ​​composited with an alloy of a transition metal with high conductivity and good catalytic activity, or with an oxide of a transition metal, or with a transition metal carbide with an electronic structure similar to that of a precious metal, or with an alloy of a transition metal and a carbide of a transition metal. The resulting integrated hydrogen evolution cathode electrode has excellent electron transport performance, gas desorption effect, hydrogen evolution catalytic activity and hydrogen evolution efficiency.

[0038] In summary, the cathode electrode of the present invention has a stable structure, a low density, a high loading amount of water electrolysis catalyst, and a high hydrogen production efficiency, which is beneficial to reducing the energy consumption of hydrogen production. The preparation process is simple and easy to operate, and the cost is low. It provides a feasible path for the large-scale and continuous promotion and application of alkaline water electrolysis hydrogen production, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a SEM (scanning electron microscope) image of the cathode electrode prepared in Example 1.

[0041] Figure 2This is the SEM image of the cathode electrode prepared in Example 3.

[0042] Figure 3 This is a comparison diagram of LSV (linear sweep voltammetry) curves of hydrogen evolution activity test of the cathode electrodes prepared in Examples 2, 5, and 6.

[0043] Figure 4 This is a stability test curve diagram of the cathode electrode prepared in Example 4. DETAILED DESCRIPTION

[0045] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.

[0046] In the following embodiments, the porosity, pore size, density and specific surface area were tested according to the standard GB T 21650.1-2008; the resistivity was tested according to the standard GB / T 1552-1995; the compressive strength was tested according to the standard GB / T 1448-2005; the contact angle was tested according to the standard ASTM D724-1999; and the relationship between the lattice constant and the degree of graphitization of the artificial graphite material was derived according to Franklin:

[0047] g=[(0.3440-c0 / 2) / 0.0086]×100%

[0048] Where g is the graphitization degree, %; c0 is the lattice constant of the c-axis of hexagonal graphite, nm. When c0=0.6708nm, g=100%; when c0=0.6880nm, g=0%. Standard QJ2507-93 specifies the method of measuring the structural parameters of carbon materials by XRD. Substituting the interplanar spacing d002 and d004 values ​​of carbon (002) and (004) measured by it into the above formula, the graphitization degree g of the sample can be calculated.

[0049] Example 1

[0050] A cathode electrode for producing hydrogen by alkaline water electrolysis is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the matrix. The specific preparation steps are as follows:

[0051] (1) Preparation of porous carbon / carbon composite matrix

[0052] (1.1) The carbon foam precursor (polyurethane sponge) is impregnated with phenolic resin. After sufficient impregnation, the excess phenolic resin is discharged and placed at 170 o C for 2 h, and then in a nitrogen atmosphere at 900 oC for 2 h, and a porous skeleton carbon with a surface covered with cracked carbon was obtained, with a density of 0.09 g / cm 3 , the porosity is 75%, and the pore size is ~230μm; it should be noted that the cracked carbon covered on the porous skeleton carbon at this time is a part of the second phase carbon (900 o C for 2 h, under which the phenolic resin is cracked at the same time), and in the subsequent steps, carbon deposition will continue on the porous skeleton carbon through a vapor deposition process to form another part of the second phase carbon;

[0053] (1.2) The porous skeleton carbon with cracked carbon on the surface obtained in step (1.1) is placed in a chemical vapor deposition furnace to continue the deposition of the second phase carbon, wherein the carbon source gas is propylene and the flow rate is 1.5 m 3 / h, deposition temperature is 900 o C, the deposition time is 80h, then another part of the second phase carbon is formed by deposition on the porous skeleton carbon; at this time, the density of the porous skeleton carbon after the deposition of the second phase carbon is 0.15g / cm 3 , the graphitization degree is 91%, and the resistivity is 38.7mΩ·cm;

[0054] (1.3) Place the porous skeleton carbon after the second phase carbon is deposited in step (1.2) into a graphitization furnace and place it in an argon protective atmosphere at 2500 o C for 1 h to obtain the porous carbon / carbon composite material matrix, with a graphitization degree of 96%, a resistivity of 11.7 mΩ·cm, and a specific surface area of ​​0.8 m 2 / g, contact angle is 140 o , compressive strength is greater than 5MPa;

[0055] (1.4) Further, the porous carbon / carbon composite material matrix obtained in step (1.3) is subjected to a roughening pretreatment, that is, the porous carbon / carbon composite material matrix is ​​placed at 550 o C for 20 min, then ultrasonically cleaned with deionized water and placed in 120 o C oven for 24 h to obtain a coarsened porous carbon / carbon composite matrix with a specific surface area of ​​1.3 m 2 / g, contact angle is 90 o ;

[0056] (2) Loading water electrolysis catalyst on porous carbon / carbon composite matrix by hydrothermal method

[0057] The roughened porous carbon / carbon composite material matrix obtained in step (1.4), 0.214 g of NiCl2·6H2O, 0.066 g of Zn(OAC)2·2H2O and 100 mL of deionized water were mixed, and after ultrasonic mixing, the mixture was transferred to a reactor and heated at 170 °C. o C for 12 h, and then cooled after the reaction. The solid product was collected and washed with deionized water and anhydrous ethanol, and finally placed in 60 o C oven for 24 hours, thereby achieving the loading of nickel zinc oxide (the molar ratio of nickel to zinc in the nickel zinc oxide is 7:3) on the porous carbon / carbon composite material matrix, and correspondingly obtaining the cathode electrode.

[0058] The specific surface area of ​​the cathode electrode prepared in Example 1 is 1.5 m 2 / g, density is 0.5g / cm 3 .

[0059] The morphology of the cathode electrode prepared in Example 1 was characterized. Figure 1 It can be seen from the SEM image that nickel-zinc oxide particles grow on the three-dimensional network skeleton of the porous carbon / carbon composite matrix. As the reaction proceeds, the grains begin to grow and grow, and the inherent properties of nanoparticle agglomeration make the catalyst evenly wrap the matrix carbon skeleton. The size of nickel-zinc oxide particles is between 50 and 500 nm, which is conducive to gas adsorption and desorption, and is conducive to improving the hydrogen evolution performance of the cathode. At the same time, SEM testing shows that the thickness of nickel-zinc oxide loaded on the porous carbon / carbon composite matrix is ​​~1μm.

[0060] The cathode electrode prepared in Example 1 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 417 mV, indicating its high hydrogen evolution activity.

[0061] The cathode electrode prepared in Example 1 was heated to 25 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 Under the current density of , it can run stably for 500h without attenuation, indicating that its structure is stable and its service life is long.

[0062] Example 2

[0063] A cathode electrode for producing hydrogen by alkaline water electrolysis is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the matrix. The specific preparation steps are as follows:

[0064] (1) Preparation of porous carbon / carbon composite matrix

[0065] (1.1) Under nitrogen atmosphere, the density is 0.6g / cm 3 900 MW carbon fiber woven fabric with a porosity of 60% and a pore size of ~300 μm o C. 2h debinding treatment to remove the sizing agent on the surface to obtain porous skeleton carbon;

[0066] (1.2) The porous skeleton carbon obtained in step (1.1) is placed in a chemical vapor deposition furnace for deposition of the second phase carbon, wherein the carbon source gas is propylene and the flow rate is 1.5 m 3 / h, deposition temperature is 900 o C, the deposition time is 50h, then the second phase carbon is deposited on the porous skeleton carbon; at this time, the density of the porous skeleton carbon after the deposition of the second phase carbon is 0.8g / cm 3 , the graphitization degree is 94%, and the resistivity is 8.9mΩ·cm;

[0067] (1.3) Place the porous skeleton carbon after the second phase carbon is deposited in step (1.2) into a graphitization furnace and place it in an argon protective atmosphere at 2500 o C for 1 h to obtain the porous carbon / carbon composite material matrix, with a graphitization degree of 99%, a resistivity of 4.6 mΩ·cm, and a specific surface area of ​​2.1 m 2 / g, contact angle is 110 o , compressive strength is greater than 5MPa;

[0068] (1.4) Further, the porous carbon / carbon composite material matrix obtained in step (1.3) is subjected to a roughening pretreatment, that is, the porous carbon / carbon composite material matrix is ​​placed at 550 o C for 20 min, then ultrasonically cleaned with deionized water and placed in 120 o C oven for 24 h to obtain a coarsened porous carbon / carbon composite matrix with a specific surface area of ​​2.5 m 2 / g, contact angle is 70 o ;

[0069] (2) Loading water electrolysis catalyst on porous carbon / carbon composite matrix by electrodeposition

[0070] 9 g of NiSO4·6H2O, 2 g of FeSO4·7H2O, 4.5 g of H3BO3, 3 g of NaCl and 2 g of Na3C6H5O7·2H2O were dissolved in 100 mL of deionized water, mixed evenly and prepared into an electrolyte solution; a nickel-iron alloy (the molar ratio of nickel to iron in the nickel-iron alloy is 4:1) was deposited on the roughened porous carbon / carbon composite material matrix obtained in step (1.4) by a constant potential deposition method to obtain the cathode.

[0071] The specific surface area of ​​the cathode electrode prepared in Example 2 is 2.8 m 2 / g, density is 1.2g / cm 3 .

[0072] The cathode electrode prepared in Example 2 was characterized in morphology. According to the SEM characterization results, the nickel-iron alloy particles were uniformly deposited on the porous carbon / carbon composite material matrix, and the particle size was ~80nm. At the same time, the SEM test showed that the thickness of the nickel-iron alloy loaded on the porous carbon / carbon composite material matrix was ~400nm.

[0073] The cathode electrode prepared in Example 2 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 345 mV, indicating that it has high hydrogen evolution activity. Figure 3 shown.

[0074] The cathode electrode prepared in Example 2 was heated to 25 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 Under the current density of , it can run stably for 500h without attenuation, indicating that its structure is stable and its service life is long.

[0075] Example 3

[0076] A cathode electrode for producing hydrogen by alkaline water electrolysis is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the matrix. The specific preparation steps are as follows:

[0077] (1) The preparation steps and process conditions of the porous carbon / carbon composite material matrix are the same as step (1) of Example 2;

[0078] (2) Loading water electrolysis catalyst on porous carbon / carbon composite matrix by vapor deposition method

[0079] In an argon atmosphere, a nickel layer with a thickness of ~100 nm is deposited on the roughened porous carbon / carbon composite material substrate obtained in step (1.4) by physical vapor deposition technology; the porous carbon / carbon composite material substrate loaded with the nickel layer is then placed in a chemical vapor deposition furnace under a hydrogen atmosphere with a propylene flow rate of 1.0 m 3 / h, deposition temperature is 900 o C, and then cooled after being deposited for 1 hour, nickel carbide is formed on the porous carbon / carbon composite material matrix, and the cathode electrode is obtained accordingly.

[0080] The specific surface area of ​​the cathode electrode prepared in Example 3 is 3.2 m 2 / g, density is 1.6g / cm 3.

[0081] The morphology of the cathode electrode prepared in Example 3 was characterized. Figure 2 It can be seen from the SEM image that the preferentially oriented nickel carbide growth tends to be perpendicular to the porous carbon / carbon composite matrix, and the deposited nickel carbide particle size is ~700nm. This structure further increases its specific surface area, which is conducive to the full reaction of the alkali solution on the cathode and improves the electrode hydrogen evolution performance. At the same time, the SEM test shows that the thickness of the nickel carbide loaded on the porous carbon / carbon composite matrix is ​​~2μm.

[0082] The cathode electrode prepared in Example 3 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 332 mV, indicating its high hydrogen evolution activity.

[0083] The cathode electrode prepared in Example 3 was o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 Under the current density of , it can run stably for 500h without attenuation, indicating that its structure is stable and its service life is long.

[0084] Example 4

[0085] A cathode electrode for producing hydrogen by alkaline water electrolysis is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the matrix. The specific preparation steps are as follows:

[0086] (1) Preparation of porous carbon / carbon composite matrix

[0087] (1.1) Under nitrogen atmosphere, the density is 0.6g / cm 3 900 MW carbon fiber woven fabric with a porosity of 60% and a pore size of ~300 μm o C. 2h debinding treatment to remove the sizing agent on the surface to obtain porous skeleton carbon;

[0088] (1.2) The porous skeleton carbon obtained in step (1.1) is placed in a chemical vapor deposition furnace for deposition of the second phase carbon, wherein the carbon source gas is propylene and the flow rate is 2m 3 / h, deposition temperature is 1000 o C, the deposition time is 50h, then the second phase carbon is deposited on the porous skeleton carbon; at this time, the density of the porous skeleton carbon after the deposition of the second phase carbon is 0.9g / cm 3 , the graphitization degree is 95%, and the resistivity is 4.3mΩ·cm;

[0089] (1.3) Place the porous skeleton carbon after the second phase carbon is deposited in step (1.2) into a graphitization furnace and place it in an argon protective atmosphere at 2800 o C for 1 h to obtain the porous carbon / carbon composite material matrix, with a graphitization degree of 99%, a resistivity of 2.0 mΩ·cm, and a specific surface area of ​​1.2 m 2 / g, contact angle is 115 o , the compressive strength is greater than 5MPa;

[0090] (1.4) Further, the porous carbon / carbon composite material matrix obtained in step (1.3) is subjected to a roughening pretreatment, that is, the porous carbon / carbon composite material matrix is ​​first placed at 600 o C for 20 min, then placed in a 15 wt.% nitric acid solution for 10 min, then ultrasonically cleaned with deionized water, and then placed in a 120 o C oven for 24 h to obtain a coarsened porous carbon / carbon composite matrix with a specific surface area of ​​2.3 m 2 / g, contact angle is 66 o ;

[0091] (2) Combining electrodeposition and vapor deposition to load water electrolysis catalysts on porous carbon / carbon composite matrix

[0092] Dissolve 9 g of NiSO4·6H2O, 2 g of FeSO4·7H2O, 4.5 g of H3BO3, 3 g of NaCl and 2 g of Na3C6H5O7·2H2O in 100 mL of deionized water, mix well and prepare an electrolyte solution; deposit a nickel-iron alloy (the molar ratio of nickel to iron in the nickel-iron alloy is 4:1) on the roughened porous carbon / carbon composite material matrix obtained in step (1.4) by constant potential deposition method;

[0093] The porous carbon / carbon composite material matrix loaded with nickel-iron alloy was treated in a 7wt.% hydrochloric acid solution for 5 min, taken out and washed to neutrality and dried, and then placed in a chemical vapor deposition furnace under a hydrogen atmosphere with a propylene flow rate of 1.0 m 3 / h, deposition temperature is 900 o C, and then cooled after deposition for 30 minutes, nickel carbide is formed on the porous carbon / carbon composite material matrix loaded with nickel-iron alloy, that is, a water electrolysis catalyst composited with nickel-iron alloy and nickel carbide is formed on the porous carbon / carbon composite material matrix (wherein the molar ratio of nickel-iron alloy to nickel carbide is 1:2), and the negative electrode is obtained accordingly.

[0094] The specific surface area of ​​the cathode electrode prepared in Example 4 is 3.6 m 2 / g, density is 1.5g / cm 3 .

[0095] The morphology of the cathode prepared in Example 4 was characterized. According to the cross-sectional SEM characterization results, a nickel-iron alloy layer and a nickel carbide layer were present on the porous carbon / carbon composite material matrix. At the same time, SEM testing showed that the total thickness of the nickel-iron alloy layer and the nickel carbide layer loaded on the porous carbon / carbon composite material matrix was ~800nm.

[0096] The cathode electrode prepared in Example 4 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 306 mV, indicating its high hydrogen evolution activity.

[0097] The cathode electrode prepared in Example 4 was heated to 25 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 Under the current density of , it can run stably for 500h without attenuation, indicating that its structure is stable and its service life is long. Figure 4 shown.

[0098] Example 5

[0099] A cathode electrode for producing hydrogen by alkaline water electrolysis is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst supported on the matrix. The specific preparation steps are as follows:

[0100] (1) The preparation steps and process conditions of the porous carbon / carbon composite material matrix are the same as step (1) of Example 2;

[0101] (2) Loading water electrolysis catalyst on porous carbon / carbon composite matrix by electrodeposition

[0102] Dissolve 9 g of NiSO4·6H2O, 8 g of FeSO4·7H2O, 4.5 g of H3BO3, 3 g of NaCl and 2 g of Na3C6H5O7·2H2O in 100 mL of deionized water, mix well and prepare an electrolyte solution; deposit a nickel-iron alloy (the molar ratio of nickel to iron in the nickel-iron alloy is 1:1) on the roughened porous carbon / carbon composite material matrix obtained in step (1.4) by a constant potential deposition method to obtain the cathode.

[0103] The specific surface area of ​​the cathode electrode prepared in Example 5 is 3.0 m 2 / g, density is 1.4g / cm 3 .

[0104] The cathode electrode prepared in Example 5 was characterized by morphology. According to the SEM characterization results, the nickel-iron alloy particles were uniformly deposited on the porous carbon / carbon composite material matrix, and the particle size was ~100nm. At the same time, the SEM test showed that the thickness of the nickel-iron alloy loaded on the porous carbon / carbon composite material matrix was ~400nm.

[0105] The cathode electrode prepared in Example 5 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 355 mV, indicating that it has high hydrogen evolution activity. Figure 3 shown.

[0106] The cathode electrode prepared in Example 5 was heated to 25 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 Under the current density of , it can run stably for 500h without attenuation, indicating that its structure is stable and its service life is long.

[0107] Example 6

[0108] Based on Example 2, except for the absence of step (1.4), the other steps and process conditions are the same as those of Example 2. That is, in Example 6, the porous carbon / carbon composite material substrate obtained in step (1.3) is not subjected to roughening pretreatment, and step (2) is to directly deposit the nickel-iron alloy on the porous carbon / carbon composite material substrate obtained in step (1.3).

[0109] The specific surface area of ​​the cathode prepared in Example 6 is 2.4 m 2 / g, density is 1.06g / cm 3 .

[0110] The cathode electrode prepared in Example 6 was heated to 80 o C. In 30wt.% potassium hydroxide lye, at 5000A / m 2 At a current density of , the hydrogen evolution overpotential of the cathode is 415 mV. Figure 3 shown.

[0111] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A cathode electrode for producing hydrogen by alkaline water electrolysis, Features: The cathode electrode is composed of a porous carbon / carbon composite material matrix and a water electrolysis catalyst loaded on the porous carbon / carbon composite material matrix; Among them, the graphitization degree of the porous carbon / carbon composite matrix is ​​90~99%, and the specific surface area is 0.7~2.5m 2 / g, contact angle is 110~160 o , compressive strength is not less than 1.6MPa.

2. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 1, Features: The porous carbon / carbon composite material substrate is subjected to roughening pretreatment before loading the water electrolysis catalyst. The roughening pretreatment can increase the specific surface area of ​​the porous carbon / carbon composite material substrate and reduce the contact angle of the porous carbon / carbon composite material substrate, thereby improving the loading effect of the water electrolysis catalyst on the porous carbon / carbon composite material substrate. Among them, the specific surface area of ​​the porous carbon / carbon composite matrix after roughening pretreatment is 1~4m 2 / g, contact angle is 60~110 o .

3. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 1, Features: The matrix of the porous carbon / carbon composite material is formed by graphitization of porous skeleton carbon and second phase carbon covering the surface of the porous skeleton carbon; Among them, the porosity of the porous skeleton carbon is 35~80%, the pore size of the porous skeleton carbon is 50~500μm, and the density of the porous skeleton carbon is 0.05~0.7g / cm 3 The density of the porous skeleton carbon covered with the second phase carbon is 0.14~1g / cm 3 .

4. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 3, Features: Porous skeleton carbon is prepared using carbon fiber braid or carbon foam as a precursor; The porous skeleton carbon prepared from carbon fiber braids has a pore size of 100~500μm, a porosity of 35~60%, and a density of 0.6~0.7g / cm 3 The density of the second phase carbon covered on the porous skeleton carbon is 0.8~1g / cm 3 In this case, the graphitization degree of the porous carbon / carbon composite matrix formed by graphitization is 96~99%, the resistivity is 1~10mΩ·cm, and the specific surface area is 1~2.5m 2 / g, contact angle is 110~150 o ; The porous skeleton carbon prepared from foam carbon has a pore size of 50~300μm, a porosity of 40~80%, and a density of 0.05~0.12g / cm 3 The density of the porous skeleton carbon covered with the second phase carbon is 0.14~0.25g / cm 3 In this case, the graphitization degree of the porous carbon / carbon composite matrix formed by graphitization is 90~97%, the resistivity is 10~20mΩ·cm, and the specific surface area is 0.7~1m 2 / g, contact angle is 130~160 o .

5. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 4, Features: The porous carbon / carbon composite material matrix prepared by porous skeleton carbon based on carbon fiber braids has a specific surface area of ​​2~4m 2 / g, contact angle is 60~90 o ; The porous carbon / carbon composite material matrix prepared by porous skeleton carbon prepared from foam carbon has a specific surface area of ​​1~2m 2 / g, contact angle is 70~110 o .

6. A cathode electrode for producing hydrogen by alkaline water electrolysis according to any one of claims 1 to 5, Features: The water electrolysis catalyst is at least one of a transition metal alloy, a transition metal oxide, and a transition metal carbide.

7. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 6, Features: The transition metal alloy is nickel-iron alloy; the transition metal oxide is nickel-zinc oxide; the transition metal carbide is nickel carbide; when the transition metal alloy, transition metal oxide and transition metal carbide are used in combination, a composite of nickel-iron alloy and nickel carbide is used.

8. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 7, Features: The molar ratio of nickel to iron in nickel-iron alloy is 7:1~1:1; the molar ratio of nickel to zinc in nickel-zinc oxide is 7:3~1:1; in the composite of nickel-iron alloy and nickel carbide, the molar ratio of nickel-iron alloy to nickel carbide is 1:(1~3).

9. A cathode electrode for producing hydrogen by alkaline water electrolysis according to claim 6, Features: The particle size of the water electrolysis catalyst supported on the porous carbon / carbon composite material matrix is ​​0.005-2 μm, and the thickness of the water electrolysis catalyst supported on the porous carbon / carbon composite material matrix is ​​0.03-5 μm.

10. A cathode electrode for producing hydrogen by alkaline water electrolysis according to any one of claims 1 to 5, Features: The specific surface area of ​​the cathode electrode is 1.1-4.2 m 2 / g, density is 0.5~1.8g / cm 3 .

Citation Information

Patent Citations

  • Method for preparing amorphous oxyhydroxide catalyst by mechanical stirring method and research on high-efficiency hydrogen production by electrolyzing water by using amorphous oxyhydroxide catalyst

    CN114082419A

  • Carbon nanotube composite hydrogen evolution catalytic membrane and preparation method thereof

    CN114717593A

  • Multi-element metal nitride heterojunction nanorod array composite electrocatalyst as well as preparation method and application thereof

    CN114892206A

  • PdRu / MOx / NF composite material and preparation method and application thereof

    CN117187873A

  • Transition metal nitride nickel-based material electrolyzed water / urea catalyst as well as preparation method and application thereof

    CN117448877A