Synthesis method and application of one-dimensional molybdenum carbide fiber with controllable crystalline phase proportion
Through the carbon fiber carbothermal reduction method and spinning method, the ratio and temperature of the carbon source and the molybdenum source are adjusted to achieve the controllable preparation of α-MoC and β-Mo2C phases, solving the problems of high preparation difficulty and high cost in the existing technology. , provides a safe, simple and efficient preparation method, suitable for applications in multi-functional fields.
Patent Information
- Application Number
- CN202410944488.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
In the preparation process of existing molybdenum carbide materials, there are problems such as difficulty in preparing α-MoC, high cost, great safety hazards and poor controllability. In particular, the difficulty of regulating two-phase mixed materials hinders their wide application in multi-functional fields.
Through the carbon fiber carbothermal reduction method, the reducing ability of the carbon source is adjusted to achieve continuous conversion of α-MoC to β-Mo2C phase. High molecular polymer is used as the carbon source, and ammonium molybdate is used as the molybdenum source. The fiber is prepared by spinning method. , control the ratio of carbon source to molybdenum source and the pre-oxidation temperature to achieve control of the proportions of different crystal phases.
It achieves the safe, simple and efficient preparation of one-dimensional molybdenum carbide fibers, reduces the difficulty and cost of material preparation, provides application foundations in different fields, avoids the use of precious metal catalysts and reducing gases, and improves the safety and safety of the preparation process. Controllability.
Smart Images

Figure CN118727199A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiber preparation, and specifically relates to a synthesis method and application of one-dimensional molybdenum carbide fiber with controllable crystal phase ratio. Background Art
[0002] As an important class of transition metal carbides, molybdenum carbide has unique chemical and physical properties due to its electronic structure similar to that of precious metals. α-MoC and β-Mo2C, as the main crystalline phases of molybdenum carbide, show remarkable versatility. For example, in the field of catalysis, carbides often have catalytic effects comparable to those of precious metals. In thermal catalytic reactions, molybdenum carbide has attracted widespread attention in the fields of chemical conversion and energy due to its excellent catalytic performance. The application of β-Mo2C in hydrogenation reactions and water-gas shift reactions is particularly prominent, and it plays a key role in the preparation of syngas and chemical energy conversion. In terms of electrochemical applications, the excellent performance of β-Mo2C in the process of hydrogen production by water electrolysis, especially in the hydrogen evolution reaction (HER), shows its importance in the field of electrocatalysis. In addition, since carbides themselves have good thermal and chemical stability, their application in the ocean also has good prospects. In recent years, the electrolysis of seawater technology has attracted widespread attention. In the seawater environment, the chloride ion-rich environment is very easy to corrode the catalyst. Thanks to the good chemical stability of molybdenum carbide and the fact that it is a good electrocatalyst, it has important application prospects in the electrolysis of seawater.
[0003] In fuel cell technology, β-Mo2C has become a potential application object for electrode materials and has broad application prospects in energy conversion technology. In addition, the superconducting properties of α-MoC at low temperatures provide an important experimental platform for the study of superconducting phenomena. In the study of high-temperature resistant materials, β-Mo2C has been valued for its high melting point and superior mechanical properties. These characteristics make β-Mo2C have significant potential in aerospace and high-temperature industrial applications. In addition, the stability of molybdenum carbide in high-temperature environments provides a key material solution for high-temperature resistant materials in high-temperature processes. The high hardness and excellent wear resistance of molybdenum carbide make it an ideal choice for manufacturing cutting tools and wear-resistant coatings. These applications not only improve the durability and efficiency of industrial equipment, but also promote innovation in the field of materials engineering. In addition to single-phase molybdenum carbide catalysts, recent studies have shown that α-MoC and β-Mo2C mixed-phase catalysts also play their own unique physical and chemical properties in many fields, further improving the performance of the use scenario. In summary, as multifunctional materials, α-MoC and β-Mo2C have demonstrated their unique application value and broad research prospects in the fields of thermal catalysis, electrocatalysis, superconductivity, heat resistance and wear resistance. Therefore, the preparation of molybdenum carbide nanomaterials with different crystal phase structures is very important.
[0004] At present, there are many problems in the preparation process of molybdenum carbide. β-Mo2C is generally considered to be the stable phase of molybdenum carbide, while α-MoC has always been regarded as the metastable phase of molybdenum carbide. There are great difficulties in the preparation process of α-MoC. For example, a mixed atmosphere of reducing gas (such as hydrogen) and gaseous carbon source (such as methane gas) is usually used. Under the catalytic action of precious metals (rhodium, platinum, palladium, etc.), high-temperature sintering of metal molybdenum sources (such as metallic molybdenum, molybdenum oxide, etc.) can obtain α-MoC. The preparation process is relatively cumbersome, and the use of mixed atmosphere brings certain safety hazards. The use of precious metals also increases the cost of preparation. Most importantly, the controllable two-phase mixed material is difficult to regulate and prepare, which hinders its exploration in the above-mentioned fields and other potential fields. Summary of the invention
[0005] The present invention provides a synthesis method and application of one-dimensional molybdenum carbide fiber with controllable crystal phase ratio. In the reaction of preparing molybdenum carbide by carbon thermal reduction of carbon fiber, continuous conversion from metastable α-MoC to stable β-Mo2C phase can be achieved by adjusting the reducing ability of carbon. The safe, simple, efficient and flexible preparation method will greatly reduce the difficulty and cost of material preparation and provide a basis for the wide application of molybdenum carbide materials in different fields.
[0006] The technical solution of the present invention is:
[0007] In the first aspect, a method for synthesizing one-dimensional molybdenum carbide fibers with controllable crystal phase ratio is disclosed. A carbon source and a molybdenum source are dissolved in a solvent to form a spinning solution, which is prepared into a fiber membrane by a spinning method and pre-oxidized under air or oxygen conditions; a carbon thermal reduction reaction occurs in an inert atmosphere, and molybdenum carbides with different crystal structures are formed by controlling the reducing ability of the carbon source to the molybdenum source; the carbon source is a high molecular polymer; the molybdenum source is one of ammonium molybdate, sodium molybdate, molybdic acid, molybdenum acetylacetonate, molybdenum powder and molybdenum oxide; the different crystal structures include a mixed structure of one phase or two phases of metastable α-MoC and stable β-Mo2C.
[0008] Preferably, controlling the reducing ability of the carbon source to the molybdenum source includes adjusting the relative content of the carbon source and the molybdenum source, specifically: when the mass ratio of the carbon source to the molybdenum source is greater than or equal to 1:1, a metastable α-MoC phase is obtained; when the mass ratio of the carbon source to the molybdenum source is less than or equal to 1:3, a stable β-Mo2C phase is obtained; when the mass ratio of the carbon source to the molybdenum source is greater than 1:3 and less than 1:1, a mixed phase of metastable α-MoC and stable β-Mo2C is obtained. Keep the content of the carbon source unchanged, and control the carbon thermal reduction ability of the unit molybdenum source by changing the amount of metal molybdenum source during the fiber preparation process. Keep the polymer content unchanged, and pre-oxidize the polymer fiber at the same temperature under air conditions. The content of the polymer remains unchanged, and by changing the content of the metal molybdenum source, the ability of the unit molybdenum source to be carbon thermally reduced is reduced, and two molybdenum carbide crystalline phases in any proportion can also be obtained continuously and accurately.
[0009] Preferably, controlling the reducing ability of the carbon source to the molybdenum source also includes adjusting the pre-oxidation temperature, specifically: when the pre-oxidation temperature is less than or equal to 260°C, a metastable α-MoC phase is obtained; when the pre-oxidation temperature is greater than or equal to 360°C and less than 600°C, a stable β-Mo2C phase is obtained, and when the pre-oxidation temperature is greater than 260°C and less than 360°C, a mixed phase of the metastable α-MoC and the stable β-Mo2C phases is obtained; first, a polymer-based fiber with a metal molybdenum source is prepared by a fiber preparation method such as electrospinning, and then the polymer fiber is pre-oxidized under air conditions, and the pre-oxidation temperature is controlled. As the pre-oxidation temperature increases, the carbon content gradually decreases, and the reducing ability decreases, so that the crystalline phase of the molybdenum carbide gradually changes from α-MoC to β-Mo2C, and pure phase α-MoC or pure phase β-Mo2C molybdenum carbide materials can also be obtained during the control process.
[0010] Preferably, controlling the reducing ability of the carbon source to the molybdenum source also includes post-oxidation treatment, specifically: using the metastable α-MoC phase to post-treat to obtain a stable β-Mo2C phase, a mixed phase of metastable α-MoC and stable β-Mo2C, when the post-oxidation temperature is between room temperature and 310°C, a mixed phase of metastable α-MoC and stable β-Mo2C is obtained, and when the post-oxidation temperature is greater than 310°C, a stable β-Mo2C phase is obtained; α-MoC (or a two-phase mixed material) is indirectly transformed into a mixed phase or a single phase of β-Mo2C by post-oxidation treatment. The prepared α-MoC fiber is subjected to post-oxidation treatment under air or oxygen conditions and re-annealing treatment under inert gas conditions to reduce the carbon content in the α-MoC sample, and the transformation of α-MoC to other crystalline phases can also be achieved. Depending on the post-oxidation treatment temperature, the purpose of continuous and precise control of the ratio of the two can also be achieved.
[0011] Preferably, the high molecular polymer is one or a mixture of polyacrylonitrile (PAN), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polylactic acid (PLA).
[0012] Preferably, the solvent is one or a mixture of N,N-dimethylformamide, water, ethanol and chloroform.
[0013] Preferably, the high voltage applied during spinning is 8-30 KV, the distance between the tip of the spinning machine and the collecting device is 8-30 cm, and the spinning time is 2-50 hours; after the spinning is completed, a polymer membrane is obtained.
[0014] Preferably, the pre-oxidation is to heat and anneal the fiber membrane in air or oxygen conditions, with a heating rate of 0.5-20°C / min, a temperature from room temperature to 600°C, and a time of 0.5-20 hours.
[0015] Preferably, the carbothermal reduction reaction is performed by annealing in an inert atmosphere at a rate of 0.5-20° C. / min to 600-1200° C. for 1-12 hours.
[0016] The second aspect discloses a method for synthesizing one-dimensional molybdenum carbide fibers with controllable crystal phase ratio and the application of the synthesized molybdenum carbide fibers in the electrolysis of seawater.
[0017] The present invention uses cheap polymer or metal molybdenum source as raw material, and only needs to undergo annealing reaction under air conditions or inert gas conditions to obtain one-dimensional molybdenum carbide nanomaterials with continuous and precisely controlled crystal phase ratio. The cheap raw materials and simple and convenient operation are conducive to the large-scale preparation of the material.
[0018] The molybdenum carbide crystal phase control mechanism involved in the present invention is based on the change in reducing ability caused by the regulation of the relative content of the carbon source and the molybdenum source, thereby realizing the controlled preparation of molybdenum carbide with different crystal phases. The preparation conditions are controlled so that when the reducing ability is strong (high carbon: molybdenum ratio), metastable α-MoC is preferentially obtained; the preparation conditions are controlled so that when the reducing ability is strong, β-Mo2C is obtained when the reducing ability is weak (low carbon: molybdenum ratio); the preparation conditions are controlled so that the reducing ability is maintained within an appropriate range (appropriate carbon: molybdenum ratio), and a two-phase mixture of metastable α-MoC and stable β-Mo2C in any proportion is obtained. The control principle diagram of the mutual transformation of the metastable α-MoC and stable β-Mo2C is shown in the figure below. Figure 1 shown.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1) The use of noble metal catalysts is avoided in the entire preparation process, the use cost is reduced, and a molybdenum carbide material free of noble metals (or other catalysts) is obtained;
[0021] 2) Avoiding the combined use of reducing gas or small molecular carbon source gas molecules, thus improving the safety of the preparation process;
[0022] 3) The method of the present invention can realize the preparation of two crystalline phases of molybdenum carbide materials in different proportions. It can obtain both the difficult-to-prepare metastable α-MoC and the β-Mo2C crystalline phase material, or prepare molybdenum carbide materials in any proportion of the two according to demand, providing a simple and efficient source for research and production in other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a control principle diagram of the mutual transformation between the metastable α-MoC and the stable β-Mo2C phases of the present invention.
[0024] Figure 2 1 and 1 are scanning electron microscope images of the polymer fiber membrane prepared in Example 1 of the present invention, wherein a) is a scanning electron microscope image at a higher magnification, and b) is a scanning electron microscope image at a lower magnification.
[0025] Figure 3 3 is a thermogravimetric curve of the polymer fiber membrane prepared in the embodiment of the present invention.
[0026] Figure 4 1 is the X-ray diffraction pattern of the molybdenum carbide material prepared in Examples 1-6 of the present invention.
[0027] Figure 5 It is the X-ray diffraction pattern of the molybdenum carbide material prepared in Examples 7-10 and Example 1 of the present invention.
[0028] Figure 6 It is the X-ray diffraction pattern of the molybdenum carbide material prepared in Examples 11-12 and Example 1 of the present invention.
[0029] Figure 7 1 is a scanning electron microscope photograph of the molybdenum carbide material prepared in Example 1 of the present invention.
[0030] Figure 8 3 is a scanning electron microscope photograph of the molybdenum carbide material prepared in Example 6 of the present invention.
[0031] Fig. 9 The β-Mo2C obtained in Example 6 of the present invention is used as a raw material to carry out a cycle performance test of electrolyzing seawater. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] Example 1
[0034] The polymer fiber membrane is prepared by electrospinning, as follows:
[0035] 1) Dissolve polyacrylonitrile (1.0 g) and molybdenum acetylacetonate (1.0 g) in N,N-dimethylformamide (10 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution;
[0036] 2) The spinning solution was prepared into a fiber membrane using the electrospinning method. The electrospinning high voltage was 16KV, the distance between the tip of the electrospinning and the collecting device was 18cm, the electrospinning time was 10 hours, and the propulsion speed of the spinning solution was 1mL / hour. After the electrospinning was completed, a light yellow polymer membrane was generated. The polymer membrane was placed in a 60°C oven and dried overnight to remove the residual solvent, and finally a uniform and soft polymer fiber membrane was obtained. The scanning electron microscope image of the polymer fiber membrane is shown in the figure below. Figure 2 As shown in the figure, the sample is in a one-dimensional fiber shape, evenly distributed, and free of other impurities; the thermogravimetric analysis results of the polymer fiber membrane are shown in Figure 3 As shown in the figure, after 260°C, as the pre-oxidation temperature increases, the carbon-containing functional groups on the polymer are oxidized by air and gradually lose weight, resulting in a decrease in the carbon content. That is, as the pre-oxidation temperature gradually increases, the carbon content gradually decreases, and the ability of carbon thermal reduction gradually decreases.
[0037] 3) Under air conditions, the temperature was raised at a rate of 5°C / min and the temperature was set at 260°C for pre-oxidation for 2 hours. In an inert gas argon atmosphere, the temperature was raised at a rate of 5°C / min and the temperature was set at 800°C for high temperature annealing for 2 hours to obtain a molybdenum carbide material composed of a metastable α-MoC phase. The scanning electron microscope image of the molybdenum carbide material is shown in the figure below. Figure 7 As shown, even after pre-oxidation and carbonization annealing, the fiber morphology can be maintained and no obvious agglomeration occurs, indicating that the carbide obtained in this treatment process is uniform and stable.
[0038] Example 2
[0039] The difference from Example 1 is that the pre-oxidation temperature in step 3) is 310° C., and the remaining preparation processes and steps are the same as those in Example 1.
[0040] Example 3
[0041] The difference from Example 1 is that the pre-oxidation temperature in step 3) is 340° C., and the remaining preparation processes and steps are the same as those in Example 1.
[0042] Example 4
[0043] The difference from Example 1 is that the pre-oxidation temperature in step 3) is 345° C., and the remaining preparation processes and steps are the same as those in Example 1.
[0044] Example 5
[0045] The difference from Example 1 is that the pre-oxidation temperature in step 3) is 350° C., and the remaining preparation processes and steps are the same as those in Example 1.
[0046] Example 6
[0047] The difference from Example 1 is that the pre-oxidation temperature in step 3) is 360°C, and the remaining preparation processes and steps are the same as those in Example 1. The scanning electron microscope image of the product is as follows Figure 8 As shown, even after a pre-oxidation treatment at a higher temperature (the same carbonization treatment as in Example 1), the fiber morphology can be maintained without obvious agglomeration, indicating that the carbide obtained in this treatment process is uniform and stable.
[0048] The molybdenum carbide materials obtained in Examples 1-6 were analyzed by X-ray diffraction. The results are as follows: Figure 4 As shown, in Example 1, under the condition of 260°C, a molybdenum carbide material composed entirely of the metastable α-MoC phase is obtained. In Examples 2-5, as the pre-oxidation temperature increases, the proportion of the α-MoC phase gradually decreases, and the proportion of the β-Mo2C phase gradually increases, until the pre-oxidation treatment at 360°C in Example 6 obtains a molybdenum carbide material composed entirely of the β-Mo2C phase. In Examples 2-5, a mixed phase of the α-MoC phase and the β-Mo2C phase is obtained in the temperature range of greater than 260°C and less than 360°C. Therefore, by selecting the pre-oxidation temperature within the temperature range of greater than 260°C and less than 360°C, the synthesis of one-dimensional molybdenum carbide fibers with any proportion of the two crystalline phases can be achieved.
[0049] Example 7
[0050] The difference from Example 1 is that step 1) is to dissolve polyacrylonitrile (1.0 g) and molybdenum acetylacetonate (0.5 g) in N,N-dimethylformamide (10 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution; the rest of the preparation process and steps are the same as Example 1.
[0051] Example 8
[0052] The difference from Example 1 is that step 1) is to dissolve polyacrylonitrile (1.0 g) and molybdenum acetylacetonate (1.5 g) in N,N-dimethylformamide (10 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution; the rest of the preparation process and steps are the same as Example 1.
[0053] Example 9
[0054] The difference from Example 1 is that step 1) is to dissolve polyacrylonitrile (1.0 g) and molybdenum acetylacetonate (2.0 g) in N,N-dimethylformamide (10 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution; the rest of the preparation process and steps are the same as Example 1.
[0055] Example 10
[0056] The difference from Example 1 is that step 1) is to dissolve polyacrylonitrile (1.0 g) and molybdenum acetylacetonate (3.0 g) in N,N-dimethylformamide (10 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution; the rest of the preparation process and steps are the same as Example 1.
[0057] The molybdenum carbide materials obtained in Examples 7-10 and Example 1 were analyzed by X-ray diffraction. The results are as follows: Figure 5 As shown, at 0.5g (Example 7) and 1g (Example 1) of low molybdenum acetylacetonate content, a molybdenum carbide material composed entirely of the metastable α-MoC phase is obtained. As the molybdenum acetylacetonate content increases, the proportion of the α-MoC phase gradually decreases, and the proportion of the β-Mo2C phase gradually increases, until the fiber membrane with a molybdenum acetylacetonate content of 3g (Example 10) is obtained. The molybdenum carbide material composed of a single phase β-Mo2C is obtained. In the above-selected molybdenum acetylacetonate mass range greater than 0.5g and less than 3g, the mass of the metal molybdenum source can be arbitrarily adjusted, and the synthesis of one-dimensional molybdenum carbide fibers with any proportion of controlled crystal phases can also be achieved.
[0058] Embodiment 11
[0059] The molybdenum carbide material composed of the metastable α-MoC phase prepared in Example 1 is used as a raw material, and then a post-oxidation treatment is performed at a temperature of 180°C for 2 hours, and a sample is obtained after cooling to room temperature; in an atmosphere of inert gas argon, the above sample is subjected to a carburization annealing treatment at 800°C for 2 hours to obtain a molybdenum carbide material.
[0060] Example 12
[0061] The molybdenum carbide material composed of the metastable α-MoC phase prepared in Example 1 was used as a raw material, and then subjected to a post-oxidation treatment at a temperature of 310°C for 2 hours, and then cooled to room temperature to obtain a sample; in an atmosphere of inert gas argon, at 800°C, the sample was carbonized annealed for 2 hours to obtain a molybdenum carbide material.
[0062] The molybdenum carbide fibers obtained in Example 11 and Example 12 were subjected to X-ray diffraction analysis. Figure 6 As shown in the figure, with the increase of post-oxidation temperature, the proportion of β-Mo2C phase increases. Under the post-oxidation condition of 310℃, a molybdenum carbide material composed entirely of β-Mo2C phase is obtained. Therefore, by setting the post-oxidation temperature between room temperature and 310℃, the synthesis of one-dimensional molybdenum carbide fibers with any proportion of the two crystal phases can be indirectly achieved.
[0063] Embodiment 13
[0064] The β-Mo2C phase molybdenum carbide obtained in Example 6 was used as a raw material to conduct a seawater electrolysis test. The raw material was cut into 0.5×0.5 cm 2 The electrode was provided and tested under alkaline natural seawater conditions using a standard three-electrode system in the electrolytic cell, using a carbon rod as the counter electrode and a mercury / mercury oxide electrode as the reference electrode.
[0065] An electrochemical workstation was used as a detection and recording device, and linear sweep voltammetry was used to detect the material performance. The initial voltage was set to -0.6V, the end voltage was -1.6V, and the scan rate was 2mV / s. The working curve was recorded. Cyclic voltammetry was used to detect and evaluate the stability of the material. Within the above voltage range, the scan rate was 100mV / s. After the cycle was completed, the linear sweep voltammetry was used again to test and evaluate the reacted material, and the working curve was recorded. The results are shown in Fig. 9 After 2000 cycles of stability testing, the performance of β-Mo2C as a catalyst remained almost unchanged even under harsh alkaline seawater conditions, indicating that β-Mo2C has good catalytic activity and stability in the electrocatalytic hydrogen production reaction of natural seawater.
[0066] Although the present invention has been described in detail by combining the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio, characterized in that: A carbon source and a molybdenum source are dissolved in a solvent to form a spinning solution, which is then prepared into a fiber membrane by a spinning method and pre-oxidized under air or oxygen conditions; then a carbon thermal reduction reaction occurs in an inert atmosphere, and molybdenum carbide with different crystal structures is formed by controlling the reducing ability of the carbon source to the molybdenum source; The carbon source is a high molecular polymer; The molybdenum source is one of ammonium molybdate, sodium molybdate, molybdic acid, molybdenum acetylacetonate, molybdenum powder and molybdenum oxide; Different crystal structures include one phase or a mixed structure of two phases of metastable α-MoC and stable β-Mo2C.
2. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: Controlling the reducing ability of the carbon source to the molybdenum source includes adjusting the relative contents of the carbon source and the molybdenum source, specifically: when the mass ratio of the carbon source to the molybdenum source is greater than or equal to 1:1, a metastable α-MoC phase is obtained; when the mass ratio of the carbon source to the molybdenum source is less than or equal to 1:3, a stable β-Mo2C phase is obtained; when the mass ratio of the carbon source to the molybdenum source is greater than 1:3 and less than 1:1, a mixed phase of the metastable α-MoC and the stable β-Mo2C phases is obtained.
3. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: Controlling the reducing ability of the carbon source to the molybdenum source also includes adjusting the pre-oxidation temperature, specifically: when the pre-oxidation temperature is less than or equal to 260°C, a metastable α-MoC phase is obtained; when the pre-oxidation temperature is greater than or equal to 360°C and less than 600°C, a stable β-Mo2C phase is obtained; when the pre-oxidation temperature is greater than 260°C and less than 360°C, a mixed phase of the metastable α-MoC and the stable β-Mo2C phases is obtained.
4. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: Controlling the reducing ability of the carbon source to the molybdenum source also includes post-oxidation treatment, specifically: using the metastable α-MoC phase to post-treat to obtain a stable β-Mo2C phase, a mixed phase of the metastable α-MoC and the stable β-Mo2C phases, when the post-oxidation temperature is between room temperature and 310°C, a mixed phase of the metastable α-MoC and the stable β-Mo2C phases is obtained, and when the post-oxidation temperature is greater than 310°C, a stable β-Mo2C phase is obtained.
5. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: The high molecular polymer is one or a mixture of polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl alcohol or polylactic acid.
6. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: The solvent is one or a mixture of N,N-dimethylformamide, water, ethanol and chloroform.
7. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: The high voltage applied during spinning is 8-30KV, the distance between the tip of the spinning machine and the collecting device is 8-30cm, and the spinning time is 2-50 hours; after the spinning is completed, a polymer film is obtained.
8. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: Pre-oxidation is to heat and anneal the fiber membrane in air or oxygen conditions, with a heating rate of 0.5-20°C / min, a temperature from room temperature to 600°C, and a time of 0.5-20 hours.
9. The method for synthesizing one-dimensional molybdenum carbide fiber with controllable crystal phase ratio according to claim 1, characterized in that: The carbon thermal reduction reaction is performed by annealing in an inert atmosphere at a rate of 0.5-20°C / min to 600-1200°C for 1-12 hours.
10. Use of the molybdenum carbide fiber synthesized by the synthesis method according to any one of claims 1 to 9 in the electrolysis of seawater.
Citation Information
Patent Citations
Method for preparing porous molybdenum carbide nanofiber by adopting electrostatic spinning
CN104357937A
Method for preparing graphene-supported molybdenum carbide nano particle composite structure by carbon thermal reaction
CN106238082A
Graded porous molybdenum carbide nanofiber as well as preparation method and application thereof
CN114438620A
Alpha moc superconductor fibres
GB1398615A