Method for producing carbon fiber bundle
By adding a polymerized silicone oil agent to the precursor fiber bundle of the carbon fiber bundle and performing flame-resistant treatment, the problems of fusion and scratch damage between single fibers are solved, the high-strength and low-pollution production of carbon fiber is achieved, and the carbon fiber is improved. physical properties.
Patent Information
- Application Number
- CN202410854966.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-01
AI Technical Summary
In the manufacturing process of carbon fiber, the fusion and scratch damage between single fibers in the flame retardant and carbonization processes lead to a reduction in fiber quality, and the silicone oil used is prone to thermal decomposition, causing pollution and hindering fiber opening, affecting the strength of the carbon fiber. and productivity.
By adding a polymerized silicone oil agent to the precursor fiber bundle and heating it in the flame retardant process, it quickly gels to prevent thermal decomposition and penetration into the fiber, thus maintaining a high fiber quality during the carbonization process. Strength and low contamination.
It can effectively prevent fusion and scratch damage between single fibers, reduce pollution, improve the strength and productivity of carbon fibers, and obtain carbon fiber bundles with excellent physical properties.
Smart Images

Figure BDA0004917852540000131 
Figure BDA0004917852540000161 
Figure BDA0004917852540000171
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with application number 202080060219.4, application date August 27, 2020, and invention name “Method for manufacturing carbon fiber bundles”. Technical Field
[0002] The present invention relates to a method for producing a carbon fiber bundle, and more particularly to a method for producing a carbon fiber bundle comprising a step of subjecting a precursor fiber bundle of carbon fibers to flame resistance treatment (refractory treatment, anti-inflammatory treatment) by a predetermined method. Background Art
[0003] Carbon fiber has excellent specific strength and specific elastic modulus. Taking advantage of its lightness and excellent mechanical properties, it is widely used in industry as a reinforcing fiber for composite with resins for aerospace purposes, sports purposes, general industrial purposes, etc.
[0004] As a method for producing carbon fiber, a method is generally used in which a precursor fiber bundle is heated in an oxidizing atmosphere at 200 to 300° C. to convert it into a flame-resistant fiber bundle, and then carbonized in an inert atmosphere. During these heat treatments using high heat, single fibers of the precursor fiber bundle fuse (melt-bond) with each other. In addition, during these steps, scratches are generated due to friction between fibers or with the production equipment, which has the problem of reducing the quality and grade (grade) of the obtained carbon fiber.
[0005] Therefore, in the flame-proofing process, in order to prevent the fusion between single fibers caused by the large amount of heat release accompanying the heat treatment and oxidation reaction, and to prevent damage caused by scratches during the process, an oil is applied to the precursor fiber bundle. As the oil, silicone oil is mostly used. However, when silicone oil is used, a part of silicone is thermally decomposed in the flame-proofing process to generate fine dust such as silicon oxide. The fine dust flies into the flame-proofing furnace and pollutes the flame-proofing furnace, so it is necessary to clean the flame-proofing furnace frequently, which significantly reduces productivity. In addition, if the fine dust pollutes the fiber bundle, the strength of the carbon fiber bundle is reduced. Furthermore, the silicone oil applied to the fiber bundle hinders the fiber opening of the fiber bundle, or the gelled silicone oil adheres to the conveying roller and guide in the flame-proofing process and the carbonization process, and the precursor fiber and the flame-proofing fiber are entangled, which sometimes causes process failure, resulting in reduced operability and reduced strength of the obtained carbon fiber. Furthermore, since the silicone oil agent permeates into the single fibers of the precursor fiber bundle, voids are formed on the surface and inside of the single fibers, and the strength of the obtained carbon fiber bundle may be reduced instead.
[0006] Various studies have been conducted to prevent damage caused by fusion and scratching between single fibers and to suppress the reduction in operability and the reduction in strength of carbon fiber bundles caused by silicone oils. As a method for suppressing the reduction in operability caused by silicone oils, for example, Patent Document 1 discloses the use of a silicone oil with a specific composition that is difficult to gel. Patent Document 2 discloses the use of a modified silicone oil that is easy to gel in a specific ratio. In addition, Patent Document 3 proposes a method for preventing the reduction in the openability of a fiber bundle by using an oil with low viscosity. However, in such an oil, the oil easily penetrates into the single fibers of the precursor fiber, so the strength of the resulting carbon fiber is insufficient.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2018-159138
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 2015-30931
[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 2012-46855 Summary of the invention
[0012] Problems to be solved by the invention
[0013] An object of the present invention is to provide a method for producing a carbon fiber bundle, which can prevent damage caused by fusion and scratching between single fibers in a flame-proofing step and a carbonization step, and produce a carbon fiber bundle having excellent physical properties.
[0014] Means for solving problems
[0015] The present inventors have found that the above-mentioned problems can be solved by applying a silicone oil agent polymerized by predetermined heating to a precursor fiber bundle in a flameproofing step of producing a carbon fiber bundle and then performing flameproofing treatment, thereby completing the present invention.
[0016] The present invention for solving the above-mentioned problems is the production method described below.
[0017] [1] A method for producing a carbon fiber bundle, comprising the following steps (b) to (e):
[0018] (b) an oil agent imparting step of imparting a silicone oil agent to the precursor fiber bundle to obtain an oil agent-attached precursor fiber bundle,
[0019] (d) a flame-resistant step of subjecting the oil-adhered precursor fiber bundle to a flame-resistant treatment to obtain a flame-resistant fiber bundle,
[0020] (e) a carbonization step of carbonizing the flame-resistant fiber bundle,
[0021] Characterized in that the silicone oil has a dry-to-touch time of less than 40 minutes at 250°C.
[0022] The invention described in [1] above is a method for producing carbon fiber, characterized in that a predetermined silicone oil agent is applied to a precursor fiber bundle of carbon fiber, the precursor fiber bundle is heated to polymerize the silicone (high molecular weight), and then flame resistant treatment is performed. The silicone oil agent used in this method has a finger-touch dry time of less than 40 minutes at 250°C, and the silicone in the silicone oil agent is rapidly polymerized and becomes a gelled state. The polymerized silicone is difficult to thermally decompose into silicon oxide in the flame resistant step. In addition, the silicone in a gelled state due to polymerization is difficult to penetrate into the single fiber of the precursor fiber.
[0023] [2] The method for producing a carbon fiber bundle according to [1] above, further comprising, before the oil agent application step, (a) a preheating step of preheating the precursor fiber bundle at 200 to 250°C.
[0024] [3] The method for producing a carbon fiber bundle according to the above [1] or [2], wherein after the oil agent imparting step and before the flame resistant step, it further comprises: (c) a heating step of heating the oil agent attached precursor fiber bundle at 150 to 200°C.
[0025] [4] The method for producing a carbon fiber bundle according to any one of [1] to [3] above, wherein the silicone oil agent is a silicone oil agent containing amino-modified silicone having reactive terminals.
[0026] [5] The method for producing a carbon fiber bundle according to any one of [1] to [4] above, wherein the silicone oil agent is an oil-in-water emulsion.
[0027] [6] A method for producing a carbon fiber bundle according to any one of [1] to [5] above, wherein the silicone oil agent contains a polyalkylene oxide alkyl ether, the polyalkylene oxide alkyl ether contains a polyalkylene oxide and an alkyl group, the polyalkylene oxide contains both ethylene oxide units and propylene oxide units, and the number of ethylene oxide units / the number of propylene oxide units in the polyalkylene oxide alkyl ether is 2 to 20.
[0028] Effects of the Invention
[0029] According to the method for producing a carbon fiber bundle of the present invention, after a predetermined silicone oil agent is applied to a precursor fiber bundle, the silicone in the silicone oil agent is rapidly polymerized and becomes a gelled state, thereby preventing damage caused by fusion and scratching between single fibers in the flame-resistant process and the carbonization process, and at the same time, a carbon fiber bundle that is not easy to contaminate the flame-resistant furnace and has excellent physical properties can be obtained. DETAILED DESCRIPTION
[0030] Hereinafter, the method for producing carbon fiber of the present invention will be described in detail.
[0031] It should be noted that in the present invention, the finger-touch drying time refers to the time from when the center of the coating surface is lightly touched with a fingertip until the fingertip is not contaminated (refer to JIS K5600-1-1). Specifically, it is measured using the test method of the embodiment described below. That is, the bottom area is 12.6 cm 2 2.0 g of silicone oil was weighed in a round aluminum cup and placed in an oven at 250°C. The sample was taken out every 5 minutes and a stainless steel rod was brought into contact with it and then separated. The heating time at 250°C required for the sample not to adhere to the stainless steel rod was defined as the dry-to-touch time. In addition, the dry-to-touch time refers to the time required for the silicone oil to reach the dry-to-touch state, and does not refer to the actual drying time of the present invention.
[0032] The method for producing a carbon fiber bundle of the present invention comprises the following steps (b) to (e):
[0033] (b) an oil agent imparting step of imparting a predetermined silicone oil agent to the precursor fiber bundle to obtain an oil agent-attached precursor fiber bundle,
[0034] (d) a flame-resistant step of subjecting the oil-adhered precursor fiber bundle to a flame-resistant treatment to obtain a flame-resistant fiber bundle,
[0035] (e) A carbonization step of carbonizing the flame-resistant fiber bundle.
[0036] Prior to the (b) oil agent application step, it is preferred to have (a) a preheating step of preheating the precursor fiber bundle at 200 to 250°C.
[0037] After the (b) oil agent applying step and before the (d) flame resistant step, it is preferred to include (c) a heating step of heating the oil agent-attached precursor fiber bundle at 150 to 200°C.
[0038] The (b) oil agent imparting step of the present invention is a step of imparting a silicone oil agent to a precursor fiber bundle to obtain an oil agent-attached precursor fiber bundle. The amount of silicone oil agent attached to the precursor fiber is preferably 0.01 to 5.0% by mass, more preferably 0.05 to 1.5% by mass, and particularly preferably 0.1 to 0.5% by mass. It should be noted that in the present invention, the amount of silicone oil agent attached refers to the amount of the effective component of the silicone oil agent attached to the precursor fiber, and the effective component of the oil agent refers to the remaining component (solid content) (%) when the oil agent is heated at 105°C for 3 hours. The amount of silicone oil agent attached can be changed by adjusting the silicone concentration in the oil agent bath or the viscosity of the oil agent bath. In addition, after imparting the silicone oil agent, the amount of silicone oil agent attached can be adjusted by adjusting the amount of silicone oil agent remaining after extrusion (squeezing).
[0039] There is no particular limitation on the method of imparting the silicone oil to the precursor fiber bundle, and known methods such as dipping, roll dipping, and spraying can be used. Among them, dipping and roll dipping are easy to impart the silicone oil uniformly, so they are preferably used. Regarding the liquid temperature of the silicone oil bath, in order to suppress the concentration change of the silicone oil and the destruction of the emulsion caused by the evaporation of the solvent, the liquid temperature of the silicone oil bath is preferably in the range of 10 to 50°C.
[0040] The amount of the active ingredient in the silicone oil bath is preferably 0.5 to 40% by mass, more preferably 1.5 to 30% by mass. Generally, the silicone content is adjusted by appropriately diluting the silicone oil containing 5 to 70% by mass of the active ingredient with water.
[0041] The silicone oil used in the present invention has a dry-to-touch time of less than 40 minutes at 250° C. The dry-to-touch time at 250° C. is preferably 38 minutes or less. The silicone oil after dry-to-touch is in a state where silicone is polymerized and uniformly gelled, and is difficult to penetrate into the fiber bundle.
[0042] By using a silicone oil with a dry-to-touch time of less than 40 minutes at 250°C, the silicone in the silicone oil crosslinks and gels quickly, thereby preventing the silicone oil from excessively penetrating into the interior of the precursor fiber bundle. When the dry-to-touch time at 250°C exceeds 40 minutes, the oil easily penetrates into the single fiber of the precursor fiber, thereby reducing the strength of the obtained carbon fiber. On the other hand, the dry-to-touch time is preferably more than 5 minutes. If it is less than 5 minutes, the silicone oil sometimes completes gelation before the water evaporates sufficiently.
[0043] The silicone contained in the silicone oil used in the present invention is an organopolysiloxane, and may also be a modified product thereof, a branched product (branched product), a partially cross-linked product, a copolymer with other molecules, etc. Specifically, dimethyl silicone, phenylmethyl silicone, methyl hydrogen siloxane, alkyl aralkyl modified silicone, fluorine modified silicone, amino modified silicone, amino modified polyether modified silicone, amide modified silicone, and their terminal reactive silicones; silicone wax, silicone resin, silicone resin oil, silicone elastomer, stearoxymethyl polysiloxane, aminomethylaminopropylsiloxane-dimethylsiloxane copolymer. Among them, amino modified silicone, amino modified polyether modified silicone, amide modified silicone, and their terminal reactive silicones are preferred, and terminal reactive amino modified silicones are particularly preferred. Examples of such silicone oils include those disclosed in Japanese Patent Application Laid-Open Nos. 2002-129016 and 2005-298689.
[0044] There is no particular restriction on the form of the silicone oil. From the perspective of operability, water is preferably used as a solvent, and an oil-in-water emulsion is preferred. As the surfactant used to form the emulsion, it is preferred that it has high dilution stability in the silicone oil bath and can be quickly demulsified after being attached to the fiber. It is not particularly limited, but it is preferred to include a nonionic surfactant. As a nonionic surfactant, polyoxyalkylene alkyl ether (polyoxyalkylene alkyl ether) is preferred. As a polyoxyalkylene alkyl ether, an ether compound containing a polyoxyalkylene (polyoxyalkylene) and an alkyl group is preferred, and the polyoxyalkylene contains an ethylene oxide unit and / or a propylene oxide unit as a repeating unit, and particularly preferably a polyoxyalkylene containing both an ethylene oxide unit and a propylene oxide unit, and an ether compound containing an alkyl group. The number of carbon atoms in the alkyl chain of the polyoxyalkylene alkyl ether is preferably 5 to 15, and more preferably 10 to 15. In addition, the number of ethylene oxide units of the polyoxyalkylene alkyl ether is preferably 1 to 100, more preferably 1 to 50, and further preferably 1 to 20. The number of propylene oxide units is preferably 1 to 100, more preferably 1 to 50, and particularly preferably 1 to 20. The number of ethylene oxide units / the number of propylene oxide units is preferably 1 to 50, more preferably 2 to 20. By using such a polyalkylene oxide alkyl ether as a surfactant, a silicone oil having a dry-to-touch time of less than 40 minutes can be obtained.
[0045] The content of the surfactant may be appropriately adjusted depending on the content of the silicone, and is usually 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, based on 100 parts by mass of the silicone.
[0046] The method for preparing the emulsion is not particularly limited, and a known method can be used, for example, the method disclosed in Japanese Unexamined Patent Publication No. 2002-129016 (particularly paragraphs 0028 to 0034 and 0041).
[0047] As the precursor fiber bundle used in the manufacturing method of the present invention, various precursor fiber bundles such as polyacrylonitrile, pitch, rayon (cellulose) can be used. Preferably, a polyacrylonitrile fiber bundle that is easy to obtain a desired carbon fiber with high strength can be used. As the polyacrylonitrile fiber bundle, a spinning solution obtained by spinning a monomer containing preferably 90% by mass or more of acrylonitrile, more preferably 95% by mass or more, and containing 10% by mass or less of other monomers alone or in a copolymerized state can be used to manufacture it. As other monomers, itaconic acid, (meth) acrylate, etc. can be exemplified. The precursor fiber is obtained by washing, drying, and stretching the raw material fiber after spinning.
[0048] The number of filaments of the precursor fiber bundle used in the present invention is preferably 1,000 to 100,000, more preferably 3,000 to 50,000. In addition, from the perspective of manufacturing efficiency, it is preferably 12,000 or more, more preferably 24,000 or more. In addition, the number of filaments per unit width is preferably 5,000 filaments / mm or less, more preferably 3,000 filaments / mm or less. If it exceeds 5,000 filaments / mm, there is a tendency for the deviation of the amount of silicone oil to become larger.
[0049] The flame-proofing step (d) in the present invention is a flame-proofing step of flame-proofing the oil-attached precursor fiber bundle to which the silicone oil agent is attached, thereby obtaining a flame-proof fiber bundle. In the present invention, the silicone in the silicone oil agent is cross-linked and polymerized (gelled) by at least the heat treatment in the flame-proofing step. Since the silicone in the silicone oil agent is rapidly gelled, it is possible to suppress the silicone oil agent from excessively penetrating into the interior of the precursor fiber, and a high-strength carbon fiber can be obtained. In the present invention, it is preferred that the oil-attached precursor fiber bundle be heat-treated before the flame-proofing step, and it is more preferred that a heating step (c) be performed by setting an independent heat treatment furnace and heating the oil-attached precursor fiber bundle at 150 to 200° C. after the silicone oil agent is applied and before the flame-proofing step.
[0050] The heating time at 150 to 200° C. is preferably 10 to 1000 seconds, more preferably 50 to 200 seconds, and even more preferably 100 to 200 seconds. In the present invention, although the dry to touch time of the silicone oil used is specified, the heating treatment does not need to be performed until the dry to touch state is reached.
[0051] In addition, it is preferred that a preheating step (a) of preheating the precursor fiber bundle to 200 to 250° C. is provided before applying the oil agent, and then the preheated precursor fiber bundle is applied with the silicone oil agent. By preheating the precursor fiber bundle before applying the oil agent, it is possible to further inhibit the silicone oil agent from penetrating into the interior of the single fiber of the precursor fiber, and it is possible to reduce the voids existing on the surface of the single fiber of the precursor fiber, so that a carbon fiber with higher strength can be obtained. In the present invention, the treatment time of the preheating step is preferably 10 to 1000 seconds, and more preferably 100 to 300 seconds. In the present invention, from the viewpoint of the strength of the obtained carbon fiber, it is preferred that the pretreatment is performed until the water vapor adsorption amount (humidity 90%) of the treated precursor fiber is 10 cc / g or less, and it is more preferred that the water vapor adsorption amount (humidity 90%) of the treated precursor fiber is 5 to 8.5 cc / g. The water vapor adsorption amount at a humidity of 90% reflects the state of the pores on the surface of the precursor fiber. The lower the water vapor adsorption amount, the fewer voids on the surface of the single fiber of the precursor fiber.
[0052] These (a) preheating step and (c) heating step may be used together. Alternatively, after applying the silicone oil, a separate heat treatment furnace may not be provided, but the heat treatment may be performed by setting the temperature of the first stage flame resistant furnace to 150 to 200°C in the flame resistant step performed in multiple stages.
[0053] Flame resistance treatment can be carried out under known conditions. For example, when PAN-based fibers are used as precursor fibers, flame resistance treatment is carried out in heated air at 200 to 260°C and within a draw ratio range of 0.85 to 1.15 for 10 to 100 minutes. Through the flame resistance treatment, a cyclization reaction is caused in the fibers to obtain flame resistance fibers with increased oxygen bonding. The flame resistance treatment can also be carried out by applying a temperature gradient so that the treatment temperature gradually increases.
[0054] According to the manufacturing method of the present invention, the silicone oil is quickly gelled by heating after applying the silicone oil. That is, since the flame-proofing process is performed after the silicone is polymerized, it is possible to suppress the thermal decomposition of the silicone into silicon oxide in the flame-proofing process. As a result, the scattering of silicon oxide in the flame-proofing furnace is suppressed. In addition, since the silicone oil is quickly gelled, the silicone oil can be kept on the surface of the single fiber and the silicone oil can be suppressed from penetrating into the inside of the single fiber. In addition, the uneven adhesion (attachment spots) of the oil on the surface of the single fiber is suppressed, and the oil can be easily applied evenly. As a result, in the flame-proofing process, the cutting of the single fiber caused by scratching, etc. can be suppressed.
[0055] The (e) carbonization step in the present invention is a carbonization step of heating the flame-resistant fiber bundle to 300° C. or higher in an inert atmosphere to carbonize the fiber bundle. Conventionally known conditions can be used for the carbonization. For example, a method of performing a first carbonization treatment at 300 to 800° C. in a nitrogen atmosphere and then performing a second carbonization treatment at 800 to 1600° C. can be exemplified. In the case of requiring a higher elastic modulus, a graphitization treatment may also be performed at 2000 to 3000° C.
[0056] According to the manufacturing method of the present invention described above, the cutting of the single yarn can be suppressed and the fuzz described later can be made 40 μg / m or less. As a result, a high-strength carbon fiber bundle having a strength of preferably 6000 MPa or more according to JIS R-7608 can be manufactured.
[0057] Example
[0058] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the examples. Components and test methods used in the present examples and comparative examples will be described below.
[0059] [Dry to touch test]
[0060] The bottom area is 12.6cm 2 Weigh 2.0 g of silicone oil in an aluminum cup and place it in an oven at 250°C. Take out the sample every 5 minutes, make the stainless steel rod contact with it and separate it. The heating time at 250°C required for the sample not to adhere to the stainless steel rod is defined as the finger touch drying time.
[0061] [OCU (Oil Adhesion Usage)]
[0062] The oil agent adhesion amount was determined by extracting the oil agent from the oil agent adhered precursor fiber bundle by Soxhlet extraction using a mixed solution of ethanol and benzene as a solvent, drying the solution containing the oil agent, and weighing the obtained solid content.
[0063] The oil-attached precursor fiber bundle was dried at 70°C for 1 hour, and about 5 g was measured (the mass at this time was defined as M1). A mixed solution of ethanol and benzene (volume ratio of 1:2) was used as a solvent, and the oil attached to the oil-attached precursor fiber bundle was subjected to solvent extraction by reflux for 4 hours according to the Soxhlet extraction method. After extraction, the precursor fiber bundle was removed, the solvent was concentrated, and the extract was transferred to a weighing bottle (the container mass was defined as M2). After drying at 105°C for 2.5 hours, the mass of the extract (M3) was measured, and the amount of oil attached was calculated using the following formula.
[0064] Oil adhesion amount [M (mass %)] = (M3-M2) / M1×100
[0065] [Number of scrapes until the flame-resistant fiber bundle is cut]
[0066] Cut the flame-resistant fiber bundle into a length of 1.0 m. Arrange 3 stainless steel needles (2 mm in diameter) at intervals of 2 cm so that the carbon fiber bundle contacts and passes through its surface at a contact angle of 135°. Pass the cut carbon fiber bundle through the stainless steel needles in a zigzag shape, apply a tension of 1.0 g / Tex to the flame-resistant fiber bundle, and reciprocate at an amplitude of 3 cm until the fiber bundle is cut due to scraping (number of reciprocating scrapings: 200 times / minute). Count the number of reciprocating times until the fiber bundle is cut. The scratchiness of the flame-resistant fiber bundle is evaluated by the number of reciprocating times until the fiber bundle is cut using the following three levels.
[0067] ○: More than 2500 times
[0068] △: 1500~2500 times
[0069] ×: Less than 1500 times
[0070] [Number of single-filament breaks of carbonized fiber]
[0071] The carbonized fiber bundle was cut into 1.0 m pieces and unfolded, and the number of cut single fibers (number of single fiber breakages) was counted visually.
[0072] The occurrence state of single fiber breakage of the carbonized fiber was evaluated using the following three levels.
[0073] ○: Less than 100 pieces / m (count / m)
[0074] △: 100~200 pieces / m
[0075] ×: more than 200 pieces / m
[0076] [Water vapor adsorption of precursor fiber]
[0077] The pore state of the fiber surface of the precursor fiber bundle before the oil treatment was evaluated by water vapor adsorption. The precursor fiber bundle was cut into a length of about 15 cm (about 0.3 g), and the water vapor adsorption of the precursor fiber bundle was measured under the following conditions using a fully automatic gas adsorption device "AUTOSORB-1" manufactured by Yuasa Ionix Co., Ltd. The water vapor adsorption value at a humidity of 90% is the value obtained at a relative pressure (P / Po) of 0.9.
[0078] Adsorbed gas: H2O
[0079] Dead volume: He
[0080] Adsorption temperature: 293K
[0081] Measuring range: relative pressure (P / Po) = 0 ~ 1.0P: measuring pressure, Po: saturated vapor pressure of H2O
[0082] [Carbon fiber strength]
[0083] The strength of the epoxy resin impregnated bundle was measured according to JIS R-7608, and the average value of the measurements was expressed five times.
[0084] [Fuzz]
[0085] Five chrome-plated stainless steel rods with a diameter of 2 mm were arranged in a zigzag pattern at intervals of 15 mm so that the carbon fiber bundles came into contact with and passed through the surface at a contact angle of 120°. The carbon fiber bundles were scraped in a zigzag pattern between the stainless steel rods.
[0086] The scraped carbon fiber bundle is sandwiched between two pieces of polyurethane sponges (bottom surface 32mm×64mm, height 10mm, weight about 0.25g), and a weight of 125g is placed on the polyurethane sponge in such a way that the load is applied to the entire surface of the polyurethane sponge. When the carbon fiber bundle is passed at a speed of 15m / min for 2 minutes, the weight of the fluff attached to the sponge is set as the scraped fluff amount.
[0087] (Manufacturing of Precursor Fiber Bundle)
[0088] A spinning stock solution prepared by dissolving 7 mass % of an acrylonitrile-based copolymer composed of 95 mass % of acrylonitrile, 4 mass % of methyl acrylate and 1 mass % of itaconic acid in an aqueous zinc chloride solution was passed through a spinning nozzle and ejected into a 25 mass % aqueous zinc chloride solution (coagulation solution) to continuously obtain a coagulated fiber bundle. The coagulated fiber bundle was washed and stretched, oiled, dried and densified, and post-stretched to obtain a precursor fiber bundle having a single fiber fineness of 0.7 dtex and a filament count of 24,000.
[0089] (Manufacture of silicone oil)
[0090] Silicone oil A:
[0091] Add kinematic viscosity of 1000mm 2 / s, 15% by mass of amino-modified silicone oil having an amine number of 0.3, 3% by mass of polypropylene oxide polyoxyethylene tridecyl ether as a surfactant (the number of carbon atoms in the alkyl chain, ethylene oxide units, and propylene oxide units are described in Table 1), and 82% by mass of ion-exchanged water were stirred using a homogenizer to prepare an O / W type emulsion to obtain an organic silicone oil agent A. The organic silicone oil agent A had a dry-to-touch time of 35 minutes at 250°C.
[0092] Silicone oil B~G:
[0093] An O / W emulsion was prepared in the same manner as in silicone oil A, except that the type of surfactant was changed as shown in Table 1, to obtain a silicone oil. The dry-to-touch time of the silicone oil at 250° C. is shown in Table 1.
[0094] [Table 1]
[0095]
[0096] (Example 1)
[0097] The precursor fiber bundle is immersed in a silicone oil bath filled with a silicone oil solution (silicone oil A) containing silicone oil at a concentration of 15% by mass, thereby imparting an oil agent. Then, after heating at 150°C for 180 seconds, it is flame-resistant at 240-250°C for 1 hour while being stretched at 1.0 times to obtain a flame-resistant fiber bundle. Then, in a nitrogen atmosphere, a carbonization treatment is performed at 300-1200°C to obtain a carbonized fiber bundle. The obtained carbonized fiber bundle is surface-treated with an aqueous ammonium sulfate solution as an electrolyte, and a sizing agent (epoxy resin) is added and dried to obtain a carbon fiber bundle.
[0098] The number of times the flame-resistant fiber bundle was scraped until it was cut was measured and found to be more than 2,500 times.
[0099] The number of single fiber breakages of the obtained carbonized fiber bundle was less than 100 fibers / m. The strength of the carbon fiber bundle was 6200 MPa and the fuzz was 33 μg / m.
[0100] (Examples 2 to 4, Comparative Examples 1 to 5)
[0101] A carbon fiber bundle was produced in the same manner as in Example 1 except that the type of oil and the amount of oil deposited were changed as shown in Table 2. The results are shown in Table 2.
[0102] In any of Examples 1 to 4 using a silicone oil with a dry-to-touch time of 35 minutes, damage to short fibers was minimal in the flame-proofing step and the carbonization step, and high-strength, high-quality carbon fibers were obtained.
[0103] (Example 5)
[0104] The precursor fiber bundle is preheated in air at 220°C for 180 seconds. Next, the preheated precursor fiber bundle is put into a silicone oil bath filled with a silicone oil solution (silicone oil A) containing silicone oil at a concentration of 15% by mass, thereby imparting the oil. The amount of oil attached is 0.4% by mass in terms of silicone. Next, it is heated at 150°C for 90 seconds. Then, while the oil-attached precursor fiber bundle is stretched, it is flame-resistant treated at 240-250°C for 1 hour to obtain a flame-resistant fiber bundle. Next, in a nitrogen atmosphere, a carbonization treatment is performed at 300-1200°C to obtain a carbon fiber bundle.
[0105] The number of times the flame-resistant fiber bundle was scraped until it was cut was measured and found to be more than 2,500 times.
[0106] The number of single fiber breakages of the obtained carbon fiber bundle was less than 100 fibers / m. In addition, the strength of the carbon fiber bundle was 6150 MPa.
[0107] (Examples 6 to 15)
[0108] A carbon fiber bundle was produced in the same manner as in Example 5 except that the preheating temperature, preheating time, heat treatment temperature, and type of oil agent of the precursor fiber bundle were changed as described in Table 3. The results are shown in Table 3.
[0109] (Example 16)
[0110] The carbon fiber bundle was produced in the same manner as in Example 5 except that the preheat treatment of the precursor fiber bundle was not performed.
[0111] [Table 2]
[0112]
[0113] [Table 3]
[0114]
Claims
1. A method for producing a carbon fiber bundle, characterized in that: The method comprises the following steps (a) to (e): (a) preheating step, preheating the precursor fiber bundle at 200-250°C, (b) an oil agent imparting step of imparting a silicone oil agent to the precursor fiber bundle to obtain an oil agent-attached precursor fiber bundle, (c) a heating step of heating the oil-adhered precursor fiber bundle at 150 to 200° C. for 10 to 1000 seconds to crosslink the silicone in the silicone oil adhering to the oil-adhered precursor fiber bundle, (d) a flame-resistant step of subjecting the oil-adhered precursor fiber bundle to a flame-resistant treatment to obtain a flame-resistant fiber bundle, (e) a carbonization step of carbonizing the flame-resistant fiber bundle, The organic silicone oil has a dry-to-touch time of less than 40 minutes at 250°C.
2. The method for producing a carbon fiber bundle according to claim 1, wherein: The silicone oil agent is a silicone oil agent containing amino-modified silicone having reactive terminals.
3. The method for producing a carbon fiber bundle according to claim 1 or 2, wherein: The organic silicone oil agent is an oil-in-water emulsion.
4. The method for producing a carbon fiber bundle according to claim 1 or 2, wherein: The silicone oil agent includes a polyalkylene oxide alkyl ether, the polyalkylene oxide alkyl ether includes a polyalkylene oxide and an alkyl group, the polyalkylene oxide includes both an ethylene oxide unit and a propylene oxide unit, and the number of ethylene oxide units / the number of propylene oxide units of the polyalkylene oxide alkyl ether is 2 to 20.