A kind of viscose-based white felt pre-oxidation method

By using a new soaking solution and multi-walled carbon nanotubes and graphene aqueous slurry of ammonium sulfate, ammonium chloride, urea and other components, and a new soaking solution and multi-step pre-oxidation treatment, the pre-oxidation of viscose-based carbon fibers in the prior art is solved. The problem of low felt rate has achieved high felt rate and stable trapezoidal structure generation, improving material performance.

CN118727437BActive Publication Date: 2024-11-15ANHUI HONGCHANG NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411231805.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-15
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

In the existing pre-oxidation process of viscose-based carbon fibers, the pre-oxygen felt rate caused by the use of diammonium hydrogen phosphate system is generally not high, about 47%, which is difficult to meet market demand.

Method used

A brand new immersion solution mixed with ammonium sulfate, ammonium chloride, urea and other components with carboxylated multi-walled carbon nanotubes and graphene aqueous slurry is used for viscose-based white felt soaking, combined with multi-step pre-oxidation treatment, to improve cellulose Macromolecules cross-link and oxidation reactions to produce preoxygen felts with high felt rates.

Benefits of technology

The felt yield rate of pre-oxygen felt was significantly improved to reach more than 57%, and the relevant performance was slightly improved after graphitization, which was better than traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a viscose-based white felt pre-oxidation method, comprising the following steps: according to weight parts, 2-4 parts of ammonium sulfate, 2-4 parts of ammonium chloride, 8-10 parts of urea, 4-6 parts of ammonium bicarbonate, 1-3 parts of carboxylated multi-walled carbon nanotube water slurry, 1-3 parts of graphene aqueous slurry, and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution; the viscose-based white felt is immersed in the above-mentioned soaking solution, and after the soaking is completed, it is dried and pre-oxidized to obtain a pre-oxidized felt with a high felt yield. Compared with the prior art, the invention has the beneficial effects of: compared with the traditional diammonium hydrogen phosphate soaking solution, the present invention develops a brand-new multi-component soaking solution, effectively prevents the generation of levoglucose, and greatly improves the felt yield of the pre-oxidized felt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber, in particular to a viscose-based white felt pre-oxidation method. Background Art

[0002] Viscose-based carbon fiber is a fibrous carbon material and an excellent carbon-reinforced material for both military and civilian use. Viscose-based carbon fiber thermal insulation material is made by weaving viscose-based raw fibers and then graphitizing them. It has low density, corrosion resistance, high temperature resistance, fatigue resistance, and low thermal expansion coefficient. It has good softness and can achieve thermal insulation effects through wrapping. It has great market potential for use in metallurgical, photovoltaic and other equipment.

[0003] The most important process in the production of viscose-based carbon fiber insulation materials is the pre-oxidation process. The degree of pre-oxidation determines the quality of the finished graphite felt. The flame retardant used in domestic pre-oxidation production is mostly diammonium hydrogen phosphate system, that is, white felt is soaked in 4%-6% diammonium hydrogen phosphate aqueous solution, and then pre-oxidized at 230-250℃ for 1-2h. The felt yield of pre-oxidized felt obtained by this method is generally not high, at about 47%. Summary of the invention

[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a viscose-based white felt pre-oxidation method.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A viscose-based white felt pre-oxidation method comprises the following steps:

[0007] Calculated by weight, 2-4 parts of ammonium sulfate, 2-4 parts of ammonium chloride, 8-10 parts of urea, 4-6 parts of ammonium bicarbonate, 1-3 parts of carboxylated multi-walled carbon nanotube aqueous slurry, 1-3 parts of graphene aqueous slurry, and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution;

[0008] The viscose-based white felt is immersed in the above-mentioned soaking liquid, and after the soaking is completed, it is dried and pre-oxidized to obtain a pre-oxidized felt with a high felt yield.

[0009] Preferably, the method comprises the following steps:

[0010] Calculated by weight, 3 parts of ammonium sulfate, 3 parts of ammonium chloride, 9 parts of urea, 5 parts of ammonium bicarbonate, 2 parts of carboxylated multi-walled carbon nanotube aqueous slurry, 2 parts of graphene aqueous slurry, and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution;

[0011] The viscose-based white felt is immersed in the above-mentioned soaking liquid, and after the soaking is completed, it is dried and pre-oxidized to obtain a pre-oxidized felt with a high felt yield.

[0012] Preferably, the weight percentage of carbon nanotubes in the carboxylated multi-walled carbon nanotube water slurry is 10%-13%.

[0013] Preferably, the weight percentage of graphene in the graphene aqueous slurry is 5%-10%.

[0014] Preferably, the soaking time of the viscose-based white felt is 10-50 minutes.

[0015] Preferably, the drying condition is: drying at 110-130° C. until the moisture content of the white felt is less than 15%.

[0016] Preferably, the pre-oxidation conditions are: pre-oxidation at 130-140°C for 3-5 min, pre-oxidation at 160-170°C for 8-12 min, pre-oxidation at 200-210°C for 10-20 min, pre-oxidation at 150-160°C for 5-15 min, and pre-oxidation at 220-240°C for 20-40 min.

[0017] Preferably, the pre-oxidation conditions are: pre-oxidation at 135°C for 4 min, pre-oxidation at 165°C for 10 min, pre-oxidation at 205°C for 15 min, pre-oxidation at 155°C for 10 min, and pre-oxidation at 230°C for 30 min.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Compared with the traditional diammonium hydrogen phosphate soaking solution, the present invention develops a new multi-component soaking solution. Ammonium sulfate, urea and other components are soaked into the surface and interior of the viscose fiber, which can swell the fiber filaments, promote dehydration reaction, and cross-link cellulose macromolecules. Carboxylated multi-walled carbon nanotubes and graphene are soaked into the interior of the fiber, which promotes intermolecular cross-linking and oxidation reactions of the viscose fiber macromolecule chains, generating a ring-shaped and thermally stable trapezoidal structure, and also effectively preventing the formation of L-glucose, greatly improving the yield of pre-oxidized felt.

[0020] 2. After being treated with the new soaking solution of the present invention, in the subsequent pre-oxidation process, the applicant found that after pre-oxidation at 200-210°C for 10-20 minutes and then cooling to 150-160°C for 5-15 minutes, the yield of the pre-oxidized felt was improved to a certain extent. This is also one of the innovative points of the present invention. DETAILED DESCRIPTION

[0021] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0022] Some of the raw materials come from the following sources:

[0023] Carboxylated multi-walled carbon nanotube aqueous slurry, Xianfeng Nano, XFWPMC-M33, XFWPMC-H-M33;

[0024] Graphene water-based slurry, Xianfeng Nano, XFDP01, XFDP05. Example 1

[0025] A viscose-based white felt pre-oxidation method comprises the following steps:

[0026] According to weight parts, 3 parts of ammonium sulfate, 3 parts of ammonium chloride, 9 parts of urea, 5 parts of ammonium bicarbonate, 2 parts of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 2 parts of graphene aqueous slurry (Xianfeng Nano, XFDP05), and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution;

[0027] The viscose-based white felt (weight 500g / m 2 ) is immersed in the above soaking solution for 30 minutes. After the soaking is completed, it is dried at 120°C until the moisture content of the white felt is less than 15%, and pre-oxidation is performed. The pre-oxidation conditions are pre-oxidation at 135°C for 4 minutes, pre-oxidation at 165°C for 10 minutes, pre-oxidation at 205°C for 15 minutes, pre-oxidation at 155°C for 10 minutes, and pre-oxidation at 230°C for 30 minutes, and a pre-oxidized felt with a felt rate of 59.6% is obtained;

[0028] The calculation formula for felt yield is: (weight of pre-oxidized felt / viscose-based white felt)*100%. Example 2

[0029] The difference between this embodiment and embodiment 1 is that:

[0030] 1 part of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 2 parts of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0031] The obtained felt rate was 58.8% pre-oxidized felt;

[0032] The rest is exactly the same as in Example 1. Example 3

[0033] The difference between this embodiment and embodiment 1 is that:

[0034] 2 parts of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 1 part of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0035] The obtained felt rate was 58.1% pre-oxidized felt;

[0036] The rest is exactly the same as in Example 1. Example 4

[0037] The difference between this embodiment and embodiment 1 is that:

[0038] 1 part of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 1 part of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0039] The obtained felt rate was 57.1% pre-oxidized felt;

[0040] The rest is exactly the same as in Example 1. Example 5

[0041] The difference between this embodiment and embodiment 1 is that:

[0042] 3 parts of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 3 parts of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0043] The obtained felt rate was 57.6% pre-oxidized felt;

[0044] The rest is exactly the same as in Example 1.

[0045] Comparative Example 1

[0046] The difference between this comparative example and Example 1 is that:

[0047] 0 parts of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 2 parts of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0048] The obtained felt rate was 51.6% pre-oxidized felt;

[0049] The rest is exactly the same as in Example 1.

[0050] Comparative Example 2

[0051] The difference between this comparative example and Example 1 is that:

[0052] 2 parts of carboxylated multi-walled carbon nanotube aqueous slurry (Xianfeng Nano, XFWPMC-M33), 0 parts of graphene aqueous slurry (Xianfeng Nano, XFDP05);

[0053] The obtained felt rate is 52.5% pre-oxidized felt;

[0054] The rest is exactly the same as in Example 1.

[0055] Comparative Example 3

[0056] The difference between this comparative example and Example 1 is that:

[0057] The pre-oxidation conditions were: 135°C for 4 min, 165°C for 10 min, 205°C for 15 min, and 230°C for 30 min.

[0058] The obtained felt rate was 56.7% pre-oxidized felt;

[0059] That is, pre-oxidation at 205°C for 15 minutes, and then directly pre-oxidation at 230°C for 30 minutes, without the step of cooling to 155°C for pre-oxidation for 10 minutes;

[0060] The rest is exactly the same as in Example 1.

[0061] Comparative Example 4

[0062] A viscose-based white felt pre-oxidation method comprises the following steps:

[0063] Calculate by weight and evenly disperse 5 parts of diammonium hydrogen phosphate and 100 parts of pure water to obtain a soaking solution;

[0064] The viscose-based white felt (weight 500g / m 2 ) is immersed in the above-mentioned soaking solution for 30 minutes. After the soaking is completed, it is dried at 120°C until the moisture content of the white felt is less than 15%, and pre-oxidation is carried out. The pre-oxidation conditions are pre-oxidation at 240°C for 90 minutes, and the pre-oxidized felt with a felt yield of 47.6% is obtained.

[0065] Results and Analysis

[0066] Comparison of Examples 1-5 shows that the yield of preoxidized felt obtained by the method of the present invention is above 57%.

[0067] By comparing Example 1, Comparative Examples 1 and 2, it can be seen that the carboxylated multi-walled carbon nanotube aqueous slurry and the graphene aqueous slurry both play an important role in improving the felt yield. Regardless of the lack of carboxylated multi-walled carbon nanotube aqueous slurry (Comparative Example 1) or the lack of graphene aqueous slurry (Comparative Example 2), the felt yield is significantly reduced. However, when the two are used at the same time, the felt yield is significantly improved, with a synergistic enhancement effect.

[0068] By comparing Example 1 and Comparative Example 3, it can be seen that after the soaking treatment, the pre-oxidation temperature setting has a certain degree of influence on the felt yield. Pre-oxidation is carried out at 205°C for 15 minutes, and then the temperature is lowered to 155°C for pre-oxidation for 10 minutes. After the pre-oxidation, the felt yield of the pre-oxidized felt is actually improved to a certain extent.

[0069] By comparing Example 1 and Comparative Example 4, it can be seen that compared with the traditional diammonium hydrogen phosphate soaking and pre-oxidation process, the pre-oxidation felt yield obtained by the pre-oxidation method of the present invention is greatly improved.

[0070] The preoxidized felt obtained in Example 1 and Comparative Example 4 was graphitized (2200° C., 1 h) to obtain graphite felt, and its relevant properties were tested, as shown in Table 1.

[0071] Table 1

[0072]

[0073] It can be seen from Table 1 that the preoxidized felt prepared by the present invention has little difference in related properties after graphitization compared with the preoxidized felt obtained by the traditional method, and even has a slight improvement.

[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for pre-oxidation of viscose-based white felt, It is characterized in that The steps include: Calculated by weight, 2-4 parts of ammonium sulfate, 2-4 parts of ammonium chloride, 8-10 parts of urea, 4-6 parts of ammonium bicarbonate, 1-3 parts of carboxylated multi-walled carbon nanotube aqueous slurry, 1-3 parts of graphene aqueous slurry, and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution; Immerse the viscose-based white felt in the soaking solution, dry it after soaking, and perform pre-oxidation to obtain a pre-oxidized felt with a high felt yield; The weight percentage of carbon nanotubes in the carboxylated multi-walled carbon nanotube water slurry is 10%-13%; The weight percentage of graphene in the graphene aqueous slurry is 5%-10%; The pre-oxidation conditions are: pre-oxidation at 130-140° C. for 3-5 min, pre-oxidation at 160-170° C. for 8-12 min, pre-oxidation at 200-210° C. for 10-20 min, pre-oxidation at 150-160° C. for 5-15 min, and pre-oxidation at 220-240° C. for 20-40 min.

2. A viscose-based white felt pre-oxidation method according to claim 1, It is characterized in that The steps include: Calculated by weight, 3 parts of ammonium sulfate, 3 parts of ammonium chloride, 9 parts of urea, 5 parts of ammonium bicarbonate, 2 parts of carboxylated multi-walled carbon nanotube aqueous slurry, 2 parts of graphene aqueous slurry, and 100 parts of pure water are mixed and dispersed uniformly to obtain a soaking solution; The viscose-based white felt is immersed in the above-mentioned soaking liquid, and after the soaking is completed, it is dried and pre-oxidized to obtain a pre-oxidized felt with a high felt yield.

3. A viscose-based white felt pre-oxidation method according to claim 1, It is characterized in that The soaking time of the viscose-based white felt is 10-50 minutes.

4. A viscose-based white felt pre-oxidation method according to claim 1, It is characterized in that The drying condition is: drying at 110-130° C. until the moisture content of the white felt is less than 15%.

5. A viscose-based white felt pre-oxidation method according to claim 1, It is characterized in that The pre-oxidation conditions are: pre-oxidation at 135° C. for 4 min, pre-oxidation at 165° C. for 10 min, pre-oxidation at 205° C. for 15 min, pre-oxidation at 155° C. for 10 min, and pre-oxidation at 230° C. for 30 min.

Citation Information

Patent Citations

  • Graphene / carbon nano tube / carbon nanofiber electrocatalyst and preparation method thereof

    CN105148892A

  • Preparation process of viscose-based carbon fiber composite material graphite felt and prepared graphite felt

    CN113774604A

  • Method for improving carbonization yield of viscose-based carbon felt

    CN113789592A

  • Superfine viscose-based carbon fiber heat insulation hard felt and preparation method thereof

    CN114836900A

  • Electro-conductive fibers with carbon nanotubes adhered thereto, electro-conductive yarn, fibers structural object, and production processes thereof