Waterproof and antifouling composite fabric and preparation method thereof
By using a composite of polyurethane acrylate adhesive layer and fluorinated polymer and silicate waterproof and stain-resistant layer in the waterproof jacket fabric, combined with γ-aminopropyltriethoxysilane modification treatment, the problem of unstable waterproof and stain-resistant performance of the fabric was solved, achieving a highly efficient waterproof and stain-resistant effect.
Patent Information
- Application Number
- CN202411107759.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-01
Abstract
Description
Technical Field
[0001] The present application relates to the field of fabrics, and in particular to a waterproof and anti-fouling composite fabric and a preparation method thereof. Background Art
[0002] With the continuous improvement of living standards, outdoor sports have gradually become a favorite activity for urban leisure groups and ordinary weekend enthusiasts. Whether it is long-distance hiking and mountaineering, or professional expeditions and ice climbing, a suitable all-weather jacket has become a must-have. However, the waterproof performance of jackets is not stable during daily use, and the surface of the jacket is easily stained and difficult to clean. Therefore, there is an urgent need to develop a waterproof and stain-resistant composite fabric. Summary of the Invention
[0003] In order to improve the waterproof and anti-fouling properties of fabrics, the present application provides a waterproof and anti-fouling composite fabric and a preparation method thereof.
[0004] In a first aspect, the present application provides a waterproof and antifouling composite fabric, which adopts the following technical solution: A waterproof and antifouling composite fabric comprises a base layer, an adhesive layer, and a waterproof and antifouling layer arranged in sequence; the raw material of the adhesive layer comprises polyurethane acrylate; the raw material of the waterproof and antifouling layer comprises the following components in parts by weight: 30 to 60 parts of a fluoride polymer, 20 to 50 parts of a silicate, and 5 to 15 parts of a cross-linking agent.
[0005] By adopting the above technical solution, polyurethane acrylate has good bonding properties, and the waterproof and antifouling layer is compounded on the base layer. The fluoride polymer makes the waterproof and antifouling layer have good waterproof properties, and the silicate makes the waterproof and antifouling layer have good antifouling properties. In addition, polyurethane acrylate itself also has certain waterproof and antifouling properties, thereby improving the waterproof and antifouling properties of the prepared fabric.
[0006] In a specific embodiment, the fluorinated polymer includes polytetrafluoroethylene, fluorinated polyurethane, or a mixture of the two.
[0007] By adopting the above technical solution, polytetrafluoroethylene and fluorinated polyurethane have better waterproof effect.
[0008] In a specific embodiment, the silicate includes a mixture of nano-silicon dioxide and nano-titanium dioxide.
[0009] By adopting the above technical solution and utilizing the composite silicate composed of nano silicon dioxide and nano titanium dioxide, a better antifouling effect is achieved.
[0010] In a specific embodiment, the method for preparing the silicate comprises the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; The nano-silicon dioxide and nano-titanium dioxide are stirred and mixed uniformly to obtain a mixture. During the stirring process, a treatment liquid is sprayed into the mixture. After the spraying is completed, the mixture is further stirred and dried to obtain silicate.
[0011] By adopting the above technical solution, γ-aminopropyltriethoxysilane is first dissolved in ethanol to obtain a treatment liquid, and then the treatment liquid is sprayed while stirring nano-silica and nano-titanium dioxide. After spraying, stirring is continued, and finally drying is performed to complete the modification of nano-silica and nano-titanium dioxide, thereby improving the dispersion performance of nano-silica and nano-titanium dioxide.
[0012] In a specific embodiment, the weight ratio of the treatment liquid to the mixed material is 1:(13-14).
[0013] By adopting the above technical solution, the ratio of the treatment liquid to the mixed material is further limited, thereby improving the modification effect of microsilica and nano titanium dioxide.
[0014] In a specific embodiment, the cross-linking agent includes one of an organic tin compound and a titanate compound.
[0015] By adopting the above technical solution and utilizing the organic tin compound and the titanate compound, the binding force of the components in the waterproof and antifouling layer can be improved, thereby improving the stability of the waterproof and antifouling layer.
[0016] In a specific embodiment, the raw materials of the base layer include polyester fiber, silicon carbide fiber, and polyester fiber.
[0017] In a second aspect, the present application provides a method for preparing a waterproof and antifouling composite fabric, which adopts the following technical solution: A method for preparing a waterproof and antifouling composite fabric comprises the following steps: Preparation of the base layer: adding polyester fiber, silicon carbide fiber, and polyester fiber to a water jet loom for weaving to obtain a base layer; preparation of the treatment agent: stirring and mixing a fluoride polymer, a silicate, and a cross-linking agent to obtain a treatment agent; Fabric treatment: first, polyurethane acrylate is coated on the base layer to form a bonding layer, then a treatment agent is coated on the bonding layer, and finally heat-setting treatment is performed to obtain a composite fabric.
[0018] By adopting the above technical solution, polyester fiber, silicon carbide fiber, and polyester fiber are first made into cloth to obtain a base layer, then fluoride polymer, silicate, and cross-linking agent are stirred to obtain a treating agent, and then polyurethane acrylate is coated on the base layer. Finally, the treating agent is applied and heat-setting treatment is performed to obtain a composite fabric with good waterproof and anti-fouling effects.
[0019] In a specific embodiment, the heat setting treatment is performed at a temperature of 150-200° C. and for a time of 0.5-5 min.
[0020] By adopting the above technical solution, the temperature and time of heat setting are further limited, which can ensure that the waterproof and antifouling layer is effectively combined with the adhesive layer.
[0021] In summary, this application includes at least one of the following beneficial technical effects: 1. The polyurethane acrylate in this application has good bonding properties, and the waterproof and antifouling layer is composited on the base layer. The fluoride polymer makes the waterproof and antifouling layer have good waterproof properties, and the silicate makes the waterproof and antifouling layer have good antifouling properties. In addition, the polyurethane acrylate itself also has certain waterproof and antifouling properties, thereby improving the waterproof and antifouling properties of the prepared fabric. 2. In this application, γ-aminopropyltriethoxysilane is first dissolved in ethanol to obtain a treatment liquid. Then, while stirring nano-silica and nano-titanium dioxide, the treatment liquid is sprayed. After spraying, stirring is continued, and finally drying is performed to complete the modification of the nano-silica and nano-titanium dioxide, thereby improving the dispersion properties of the nano-silica and nano-titanium dioxide. 3. The method of the present application is to first make a cloth of polyester fiber, silicon carbide fiber, and polyester fiber to obtain a base layer, then stir a fluoride polymer, a silicate, and a cross-linking agent to obtain a treating agent, and then coat polyurethane acrylate on the base layer, and finally coat the treating agent and perform heat setting treatment to obtain a composite fabric with good waterproof and antifouling effects. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments.
[0023] All raw materials in the examples are commercially available.
[0024] Preparation Example Preparation Example 1 Preparation Example 1 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; Nano-silicon dioxide and nano-titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, the treatment liquid is slowly sprayed into the mixture. After the spraying is completed, stirring is continued for 0.5 hours. Finally, the mixture is dried at 100°C for 1 hour to obtain silicate; wherein the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; the weight ratio of the treatment liquid to the mixture is 1:12.5.
[0025] Preparation Example 2 Preparation Example 2 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; Nano-silicon dioxide and nano-titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, the treatment liquid is slowly sprayed into the mixture. After the spraying is completed, stirring is continued for 0.5 hours. Finally, the mixture is dried at 100°C for 1 hour to obtain silicate; wherein the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; and the weight ratio of the treatment liquid to the mixture is 1:13.
[0026] Preparation Example 3 Preparation Example 3 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; Nano-silicon dioxide and nano-titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, the treatment liquid is slowly sprayed into the mixture. After the spraying is completed, stirring is continued for 0.5 hours. Finally, the mixture is dried at 100°C for 1 hour to obtain silicate; wherein the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; the weight ratio of the treatment liquid to the mixture is 1:13.5.
[0027] Preparation Example 4 Preparation Example 4 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; Nano-silicon dioxide and nano-titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, the treatment liquid is slowly sprayed into the mixture. After the spraying is completed, stirring is continued for 0.5 hours. Finally, the mixture is dried at 100°C for 1 hour to obtain silicate; wherein the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; and the weight ratio of the treatment liquid to the mixture is 1:14.
[0028] Preparation Example 5 Preparation Example 5 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; Nano-silicon dioxide and nano-titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, the treatment liquid is slowly sprayed into the mixture. After the spraying is completed, stirring is continued for 0.5 hours. Finally, the mixture is dried at 100°C for 1 hour to obtain silicate; wherein the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; the weight ratio of the treatment liquid to the mixture is 1:14.5.
[0029] Preparation Example 6 Preparation Example 6 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; The nano-silica was mixed evenly, and the treatment liquid was slowly sprayed into the nano-silica during the stirring process. After the spraying was completed, the stirring was continued for 0.5 hours, and finally the mixture was dried at 100° C. for 1 hour to obtain silicate; wherein the weight ratio of the treatment liquid to the nano-silica was 1:13.5.
[0030] Preparation Example 7 Preparation Example 7 provides a method for preparing silicate, comprising the following steps: γ-aminopropyltriethoxysilane, ethanol, and water are stirred and mixed to obtain a treatment solution; wherein the weight ratio of γ-aminopropyltriethoxysilane, ethanol, and water is 5:18:2; The nano titanium dioxide was stirred and mixed evenly. During the stirring process, the treatment liquid was slowly sprayed into the nano titanium dioxide. After the spraying was completed, the stirring was continued for 0.5 hours. Finally, the mixture was dried at 100°C for 1 hour to obtain silicate. The weight ratio of the treatment liquid to the nano titanium dioxide was 1:13.5. Example
[0031] Example 1 Example 1 provides a method for preparing a waterproof and antifouling composite fabric, comprising the following steps: Preparation of the base layer: polyester fiber, silicon carbide fiber, and polyester fiber are added to a water jet loom for weaving, and then shaped to obtain a base layer; wherein the weight ratio of the polyester fiber, silicon carbide fiber, and polyester fiber is 1:0.3:0.02; Preparation of a treatment agent: 30 kg of a fluoride polymer, 20 kg of a silicate, and 5 kg of a cross-linking agent are stirred and evenly mixed to obtain a treatment agent; wherein the fluoride polymer is fluorinated polyurethane; the silicate is a mixture of nano-silicon dioxide and nano-titanium dioxide, and the weight ratio of the nano-silicon dioxide to the nano-titanium dioxide is 1:1; the cross-linking agent is a titanate compound, and the titanate compound is tetraisopropyl titanate; Fabric treatment: first, polyurethane acrylate is coated on the base layer to form a bonding layer with a thickness of 1 micron, then a treatment agent is coated on the bonding layer to obtain a waterproof and antifouling layer with a thickness of 3 microns, and finally a heat setting treatment is performed at 150°C for 5 minutes to obtain a composite fabric.
[0032] Example 2 The difference between Example 2 and Example 1 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of silicate, and 10 kg of cross-linking agent are stirred and mixed uniformly to obtain the treatment agent; wherein the fluoride polymer is fluorinated polyurethane; the silicate is a mixture of nano-silica and nano-titanium dioxide, and the weight ratio of nano-silica to nano-titanium dioxide is 1:1; the cross-linking agent is a titanate compound, and the titanate compound is tetraisopropyl titanate; the remaining steps are consistent with Example 1.
[0033] Example 3 The difference between Example 3 and Example 1 is that, in preparing the treatment agent, 60 kg of fluoride polymer, 50 kg of silicate, and 15 kg of cross-linking agent are stirred and mixed uniformly to obtain the treatment agent; wherein the fluoride polymer is fluorinated polyurethane; the silicate is a mixture of nano-silicon dioxide and nano-titanium dioxide, and the weight ratio of nano-silicon dioxide to nano-titanium dioxide is 1:1; the cross-linking agent is a titanate compound, and the titanate compound is tetraisopropyl titanate; the remaining steps are consistent with Example 1.
[0034] Example 4 The difference between Example 4 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 1, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0035] Example 5 The difference between Example 5 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 2, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0036] Example 6 The difference between Example 6 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 3, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0037] Example 7 The difference between Example 7 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 4, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0038] Example 8 The difference between Example 8 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 5, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0039] Example 9 The difference between Example 9 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 6, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0040] Example 10 The difference between Example 10 and Example 2 is that, in preparing the treatment agent, 45 kg of fluoride polymer, 35 kg of the silicate prepared in Preparation Example 7, and 10 kg of the cross-linking agent were stirred and mixed uniformly to obtain the treatment agent; the remaining steps were consistent with Example 2.
[0041] Example 11 The difference between Example 11 and Example 6 lies in the fabric treatment: first, polyurethane acrylate is coated on the base layer to form a bonding layer with a thickness of 1 micron, then a treatment agent is coated on the bonding layer to obtain a waterproof and antifouling layer with a thickness of 3 microns, and finally, heat setting treatment is performed at 175°C for 2.5 minutes to obtain a composite fabric; the remaining steps are consistent with Example 6.
[0042] Example 12 The difference between Example 12 and Example 6 is that, in the fabric treatment, polyurethane acrylate is first coated on the base layer to form a bonding layer with a thickness of 1 micron, and then a treatment agent is coated on the bonding layer to obtain a waterproof and antifouling layer with a thickness of 3 microns, and finally a heat setting treatment is performed at 200°C for 0.5 minutes to obtain a composite fabric; the remaining steps are consistent with Example 6.
[0043] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the fabric is treated; a treatment agent is applied on the base layer to obtain a waterproof and antifouling layer with a thickness of 4 microns, and finally a heat setting treatment is performed at 150°C for 5 minutes to obtain a composite fabric; the remaining steps are consistent with Example 1.
[0044] Performance testing test Waterproof performance: According to GB / T4744 "Testing and evaluation of waterproof performance of textiles", the fabrics in each embodiment and comparative example were tested to obtain a waterproof grade of 0-5, with grade 0 being no waterproof performance and grade 5 being extremely waterproof performance.
[0045] Antifouling performance: The fabrics in each embodiment and comparative example were tested in accordance with GB / T 30159.1-2013 "Testing and Evaluation of Antifouling Performance of Textiles Part 1: Stain Resistance" to obtain the contact angle. The larger the contact angle, the better the antifouling performance of the fabric.
[0046] Table 1 Fabric performance test results sample Waterproof grade Contact angle (°) Example 1 4 87.1 Example 2 4 87.6 Example 3 4 87.3 Example 4 5 90.2 Example 5 5 93.2 Example 6 5 93.4 Example 7 5 93.1 Example 8 5 90.5 Example 9 5 91.5 Example 10 5 91.8 Example 11 5 94.5 Example 12 5 94.0 Comparative Example 1 3 85.5 Combining Examples 1-3 and Comparative Example 1, the fabrics in Examples 1-3 have better waterproof and antifouling properties. It can be seen that when the base layer is subjected to waterproof and antifouling treatment, the waterproof and antifouling layer and the base layer are compounded using polyurethane acrylate, which can further improve the waterproof and antifouling properties of the fabric.
[0047] Combining Example 2 and Example 4, the waterproof and antifouling properties of the fabric in Example 4 are better. It can be seen that the silicate uses modified nano-silica and nano-titanium dioxide, and the dispersion performance of nano-silica and nano-titanium dioxide is better. The γ-aminopropyltriethoxysilane on the surface can further improve the binding force of the components in the waterproof and antifouling layer, thereby further improving the waterproof and antifouling properties of the fabric.
[0048] Combined with Examples 4-8, the waterproof and antifouling properties of the fabrics in Examples 5-7 are better. It can be seen that when the mixture composed of nano-silicon dioxide and nano-titanium dioxide is modified, the ratio of the treatment liquid to the mixture is preferably 1: (13-14), which has a better modification effect on the mixture, thereby improving the waterproof and antifouling properties of the fabric.
[0049] Combining Example 6, Example 9 and Example 10, the antifouling performance of the fabric in Example 6 is the best, which shows that the silicate is preferably a mixture of nano-silicon dioxide and nano-titanium dioxide, and the performance of the waterproof and antifouling layer obtained is better.
[0050] Combining Example 6, Example 11 and Example 12, the antifouling performance of the fabric in Example 11 is the best. It can be seen that when the fabric is subjected to heat setting treatment, the treatment conditions in Example 11 are the best, thereby obtaining the best waterproof and antifouling performance of the fabric.
[0051] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A waterproof and anti-fouling composite fabric, Features: The invention comprises a base layer, an adhesive layer and a waterproof and antifouling layer which are arranged in sequence; the raw material of the adhesive layer comprises polyurethane acrylate; the raw material of the waterproof and antifouling layer comprises the following components in parts by weight: 30-60 parts of fluoride polymer, 20-50 parts of silicate and 5-15 parts of crosslinking agent.
2. A waterproof and antifouling composite fabric according to claim 1, Features: The fluoride polymer includes one of polytetrafluoroethylene and fluorinated polyurethane or a mixture of the two.
3. The waterproof and antifouling composite fabric according to claim 1, Features: The silicate comprises a mixture of nano silicon dioxide and nano titanium dioxide.
4. A waterproof and antifouling composite fabric according to claim 3, Features: The preparation method of the silicate comprises the following steps: Stir and mix γ-aminopropyltriethoxysilane, ethanol and water to obtain a treatment solution; The nano silicon dioxide and nano titanium dioxide are stirred and mixed evenly to obtain a mixture. During the stirring process, a treatment liquid is sprayed into the mixture. After the spraying is completed, the mixture is continuously stirred and dried to obtain silicate.
5. A waterproof and antifouling composite fabric according to claim 4, Features: The weight ratio of the treatment liquid to the mixed material is 1:(13-14).
6. The waterproof and antifouling composite fabric according to claim 1, Features: The cross-linking agent includes one of an organic tin compound and a titanate compound.
7. The waterproof and antifouling composite fabric according to claim 1, Features: The raw materials of the base layer include polyester fiber, silicon carbide fiber and terylene fiber.
8. A method for preparing the waterproof and antifouling composite fabric according to any one of claims 1 to 7, Features: The following steps are involved: Preparation of base layer: adding polyester fiber, silicon carbide fiber and polyester fiber into a water jet loom for weaving to obtain a base layer; Preparing a treating agent: stirring and mixing the fluoride polymer, silicate and cross-linking agent to obtain a treating agent; Fabric treatment: firstly, polyurethane acrylate is coated on the base layer to form a bonding layer, then a treatment agent is coated on the bonding layer, and finally a heat setting treatment is performed to obtain a composite fabric.
9. The method for preparing a waterproof and antifouling composite fabric according to claim 8, Features: During the heat setting treatment, the temperature is 150-200° C. and the time is 0.5-5 min.