Wood material abrasive belt grinding surface generation evaluation and comparison method

The sliding scratch test is used to evaluate the proportion of sliding, compacting, plowing and cutting behaviors of the abrasive belt on wooden materials, which solves the problem of lack of evaluation methods in the existing technology and improves grinding efficiency and energy utilization.

CN118730781APending Publication Date: 2024-10-01ZHEJIANG FORESTRY UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410719203.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology lacks effective methods to evaluate and compare the surface creation of abrasive belt grinding of wooden materials, making it difficult to select an appropriate abrasive belt type and affecting processing efficiency and energy utilization.

Method used

The sliding and scratching test is used to evaluate the proportion of sliding, compacting, plowing and cutting behaviors of the abrasive belt on wooden materials. The sliding and scratching test device is used to measure, and the comprehensive score is calculated through normalization processing to guide the selection of abrasive belts.

Benefits of technology

It provides a scientific evaluation method for the surface creation of abrasive belt grinding of wooden materials, improves the energy utilization and efficiency of the grinding process, and is suitable for the processing of different wooden materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730781A_ABST
    Figure CN118730781A_ABST
Patent Text Reader

Abstract

The invention discloses a wood material abrasive belt grinding surface generation evaluation comparison method, and relates to the technical field of wood material grinding, the method comprises the following steps: S1, preparing a wood material sample and a page type abrasive belt strip, and measuring initial values; s2, carrying out a sliding scratch test; s3, the average tangential force delta r is measured and compared; s4, measuring and comparing the average density variation delta d of the surface layer area of the wood material sample; s5, measuring and comparing the interface expansion area ratio Sdr of the wood material sample; s6, measuring and comparing the material removal rate delta c of the wood material sample; and S7, performing normalization processing on the evaluation value, and calculating a comprehensive score CS according to a set weight. By means of the method, comparison and comprehensive evaluation can be conducted on the wood material abrasive belt grinding surface generation behaviors. The sliding scratching device provided by the invention is compact in structure, the wood material sample and the page type abrasive belt strip are convenient to disassemble and assemble, the normal load and the moving speed are adjustable, and the creation process of the grinding surface of the wood material abrasive belt under different parameters can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wood material grinding, in particular to a method for evaluating and comparing the surface creation of wood material sand belt grinding. Background Art

[0002] Belt grinding plays an important role in the mechanical processing of wood materials such as wood, bamboo, and artificial boards. The belt grinding process of wood materials is mainly reflected in the comprehensive action of a large number of abrasive units on the grinding tool to complete a certain amount of material removal and generate a new surface with certain microscopic morphological characteristics and surface roughness structure. The grinding surface creation process of wood materials mainly includes sliding, compacting, plowing, and cutting behaviors. Among them, the sliding behavior is mainly manifested as the friction between the abrasive and the workpiece material, as well as the elastic deformation and recovery of the workpiece material; because the wood material has a porous structure, under the action of grinding pressure, a certain thickness of surface dense layer is formed; the plowing behavior of the abrasive will leave deep and shallow furrows on the workpiece surface; the cutting behavior is mainly manifested as the destruction and separation of the workpiece material and the formation of chips. Among them, sliding, compacting, and plowing behaviors do not directly cause the cutting removal of the workpiece material. Therefore, from the perspective of energy utilization, the smaller the proportion of sliding, compacting, and plowing behaviors in the grinding surface creation stage, the greater the proportion of cutting behaviors, and the higher the energy utilization rate of the grinding process.

[0003] Existing research on the surface creation of wood materials grinding is mostly theoretical, such as using a single abrasive grain to simulate the negative rake cutting process during grinding, and lacks a method for evaluating and comparing the surface creation of macroscopic abrasive belt grinding. In actual production, there are many types of abrasive belts, and there is currently no mature and reliable method for how to choose the appropriate abrasive belt type for different wood materials. Most of them are based on experience and theoretical analysis.

[0004] Therefore, in order to improve the level of green processing of wood materials, especially to improve the efficiency and energy utilization of abrasive belt grinding of wood materials, a feasible method for evaluating and comparing the surface creation of abrasive belt grinding of wood materials is needed in production applications, so as to select suitable abrasive belt products for specific processed objects. Summary of the invention

[0005] The purpose of the present invention is to provide a method for evaluating and comparing the surface creation of wood materials by abrasive belt grinding, so as to solve the problems existing in the above-mentioned prior art. By evaluating the proportion of sliding, compacting, plowing and cutting behaviors, an evaluation and comparison basis is provided for the processing effects of different types of abrasive belts on different wood materials, thereby improving the energy utilization rate in the grinding process.

[0006] To achieve the above object, the present invention provides the following scheme: The present invention provides a method for evaluating and comparing the surface creation of a wood material by abrasive belt grinding, comprising the following steps:

[0007] S1: cutting wood material samples and leaf abrasive strips, weighing the initial mass of the wood material samples, and determining the initial cross-sectional density of the wood material samples;

[0008] S2: Sliding scratch test on wood material and leaf abrasive belt strips under the same normal load, moving speed and moving distance;

[0009] S3: Compare the measured average tangential force δ r Size, average tangential force δ r The larger one indicates that the “slip and rub” behavior accounts for a larger proportion;

[0010] S4: Measure the cross-sectional density of the wood material sample again, obtain its density distribution in the thickness direction, and compare the average density change δ of the surface area of ​​the sample d , the average density change δ d The larger one indicates that the proportion of “dense” behavior is larger;

[0011] S5: Determine the interface extension area ratio Sdr of the scratched surface of the wood material sample. A larger Sdr indicates a larger proportion of "ploughing" behavior;

[0012] S6: Weigh the mass of the wood material sample again, calculate the difference with the initial mass, and divide the mass difference by the initial mass of the sample to obtain the material removal rate δ c , material removal rate δ c The larger one indicates that the “cutting” behavior accounts for a larger proportion;

[0013] S7: Normalize the above evaluation values, where the interface expansion area ratio Sdr and material removal rate δ c The result is a percentage, which can be used directly as a normalized value, δ r_ normalized=δ r / δ r _max, where δ r _max is the maximum tangential force value during the test, δ d _normalized = δ d / δ d _max, where δ d _max is the maximum density of the surface layer during the test. According to the requirements for the grinding results, the weights of sliding, compacting, plowing, and cutting behaviors are set to R, D, P, and C, respectively. The normalized values ​​are used to calculate the comprehensive score CS, that is, CS = (δ r _normalized*R)+(δ d _normalized*D)+(Sdr*P)+(δ c *C), a high overall score is a positive evaluation result.

[0014] Preferably, in step S1, the wood material sample and the leaf-type abrasive belt strip are cut by sawing or shearing.

[0015] Preferably, in step S4, the cross-sectional density is determined by X-ray cross-sectional density measurement, and the surface area is determined based on a critical change in a density distribution curve.

[0016] Preferably, in step S5, the interface extension area ratio Sdr is measured by a light section method or a laser triangulation method.

[0017] The present invention also provides a sliding scratch test device used in the above method, comprising a sample clamping mechanism, a sanding belt clamping mechanism, a normal loading mechanism, and a unidirectional force measuring device. The frame of the sample clamping mechanism is provided with a threaded through hole, and the sample is locked by a screw. The sanding belt clamping mechanism and the normal loading mechanism are an integral whole. The sanding belt clamping mechanism comprises a fastening screw and a belt loading area, and the fastening screw is used to fasten the two ends of the leaf sanding belt strip. The normal loading mechanism can adjust the size of the normal load by changing the mass and quantity of the added weights. The unidirectional force measuring device comprises a spring, a mechanical sensor, a cantilever bracket and a chuck. The spring plays a role in accurately measuring the tangential force during the period from stationary to relative displacement of the wood material sample and the leaf sanding belt strip. The cantilever bracket can be driven by a motor to move within a certain range along the horizontal slide rail inside the body, and the speed is adjustable. A cylindrical through hole is provided on the chuck.

[0018] Preferably, the abrasive belt clamping mechanism and the normal loading mechanism are integrally connected to the circular hole on the clamping head via a connecting rod and a clamping column.

[0019] Preferably, the connecting rod and the clamping column are connected by threads, and the clamping column of a suitable length can be selected according to the dimensional change of the wood material sample in the thickness direction.

[0020] Compared with the prior art, the present invention has achieved the following technical effects:

[0021] The present invention provides a method for evaluating and comparing the surface creation of wood materials by belt grinding. The method compares and comprehensively evaluates the proportions of "sliding", "compacting", "ploughing" and "cutting" behaviors in the process of surface creation of wood materials by belt grinding. By using the sliding scratch test device provided by the present invention, the preparation of wood material samples and page-type sanding belt strips is simple, the normal load can be easily adjusted, and the sliding scratch test of wood material samples of different sizes under different parameter conditions can be adapted. The physical quantity measurement method for judgment is mature, and the evaluation and comparison method conforms to the grinding surface creation characteristics of wood materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 A flow chart of a method for evaluating and comparing the surface creation of a wood material by abrasive belt grinding according to the present invention;

[0024] Figure 2 It is a front view of the main body of the sliding scratch testing device of the present invention;

[0025] Figure 3 It is a top view of the main body of the sliding scratch testing device of the present invention;

[0026] Figure 4 It is a front view of the entire abrasive belt clamping mechanism and normal loading mechanism in the sliding scratch testing device of the present invention;

[0027] Figure 5 It is a top view of the entire abrasive belt clamping mechanism and normal loading mechanism in the sliding scratch testing device of the present invention;

[0028] Among them, 1. power switch; 2. human-computer interaction interface; 3. cantilever bracket; 4. mechanical sensor; 5. spring; 6. chuck; 7. sample loading area; 8. locking screw; 9. clamping column; 10. connecting rod; 11. belt loading area; 12. fastening screw; 13. load area A; 14. load area B. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The purpose of the present invention is to provide a method for evaluating and comparing the surface creation of wood materials by abrasive belt grinding, so as to solve the problems existing in the above-mentioned prior art. Through the sliding scratch test process, the main proportion of the surface creation of wood materials can be determined, thereby guiding the selection of suitable abrasive belt products for different processed objects, and evaluating the surface creation of various coated abrasives, and further analyzing their grinding characteristics.

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] Please refer to Figures 1 to 5 As shown, a method for evaluating and comparing the surface creation of a wood material by belt grinding is provided, comprising the following steps:

[0033] S1: Prepare wood material sample specifications and various types of leaf abrasive strips by sawing or shearing, weigh the initial weight of the wood material sample using a precision balance, and measure the initial cross-sectional density of the wood material sample in the thickness direction using an X-ray cross-sectional density meter;

[0034] S2: Sliding scratch test on wood material specimens and various types of leaf abrasive strips under the same normal load, moving speed and moving distance;

[0035] S3: Compare the measured average tangential force δ r Size, average tangential force δ r A larger value indicates that the “slippage” behavior accounts for a larger proportion, which is manifested as more friction phenomena, elastic deformation and recovery of the material;

[0036] S4: Use the X-ray profile density meter to measure the cross-sectional density of the wood material sample again, obtain its density distribution in the thickness direction, and compare the average density change δ of the surface area of ​​the sample d , the average density change δ d The larger one indicates that the “densified” behavior accounts for a larger proportion, and a more obvious densified layer appears;

[0037] S5: Using a three-dimensional profilometer based on the optical section method, the interface expansion area ratio Sdr of the scratched surface of the wood material sample is measured. A larger Sdr indicates a larger proportion of "ploughing" behavior, leaving more furrows and material ridges on the sample surface;

[0038] S6: Use a precision balance to weigh the wood material sample again, calculate the difference from the initial weight, and divide the mass difference by the initial mass of the sample to obtain the material removal rate δ c , material removal rate δ c A larger value indicates that the “cutting” behavior accounts for a larger proportion, resulting in more material removal, which is a key indicator of grinding effect from the perspective of energy utilization;

[0039] S7: Normalize the above evaluation values, where the results of the interface expansion area ratio Sdr and the material removal rate are percentages, which can be directly used as normalized values, δ r _normalized = δ r / δ r _max, where δ r _max is the maximum tangential force value during the test, δ d _normalized = δ d / δd _max, where δ d _max is the maximum density of the surface layer during the test. The actual removal of the material is taken into consideration. The weights of sliding, compacting, plowing, and cutting behaviors are set to 10%, 15%, 15%, and 60%, respectively. The normalized values ​​are used to calculate the comprehensive score, CS = (δ r _normalized*0.1)+(δ d _normalized*0.15)+(Sdr*0.15)+(δ c *0.6), at this time, the large comprehensive score indicates that the comprehensive cutting ability is strong, the grinding efficiency is high, and the grinding process is stable.

[0040] In step S2, the sliding scratch device used for the sliding scratch test includes a power switch 1, a human-machine interface 2, a sample clamping mechanism, an abrasive belt clamping mechanism, a normal loading mechanism and a unidirectional force measuring device.

[0041] A threaded through hole is provided on the frame of the sample clamping mechanism, and the wood material sample is placed in the sample loading area 7 and fastened with a locking screw 8 .

[0042] The abrasive belt clamping mechanism and the normal loading mechanism are integrated into one, and the abrasive belt clamping mechanism comprises a fastening screw 12 and a belt loading area 11 formed by a plane and an arc surface transition zone, and the fastening screw 12 is used to fasten both ends of the leaf abrasive belt strip.

[0043] The normal loading mechanism includes a load A zone 13 and a load B zone 14, and the size of the normal load can be adjusted by changing the mass and quantity of the added weights.

[0044] Among them, the unidirectional force measuring device includes a spring 5, a mechanical sensor 4, a cantilever bracket 3 and a chuck 6. The spring 5 plays a role in accurately measuring the tangential force during the period from static to relative displacement of the wood material sample and the leaf sanding belt strip. The cantilever bracket 3 can be driven by a motor and move within a certain range along the horizontal slide rail inside the body with adjustable speed. A cylindrical through hole is opened on the chuck 6.

[0045] The abrasive belt clamping mechanism and the normal loading mechanism are integrally connected to the circular hole on the clamping head 6 via a connecting rod 10 and a clamping column 9 .

[0046] The connecting rod 10 is connected to the clamping column 9 by threads, and the clamping column 9 of a suitable length can be selected according to the size change of the wood material sample in the thickness direction.

[0047] Adaptive changes made according to actual needs are all within the protection scope of the present invention.

[0048] It should be noted that it is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any reference numerals in the claims should not be regarded as limiting the claims involved.

[0049] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for evaluating and comparing the surface creation of wood materials by belt grinding, characterized in that: The following steps are involved: S1: cutting wood material samples and leaf abrasive strips, weighing the initial mass of the wood material samples, and determining the initial cross-sectional density of the wood material samples; S2: Sliding scratch test on wood material and leaf abrasive belt strips under the same normal load, moving speed and moving distance; S3: Compare the measured average tangential force δ r Size, average tangential force δ r A larger value indicates that the "slipping" behavior accounts for a larger proportion; S4: Measure the cross-sectional density of the wood material sample again, obtain its density distribution in the thickness direction, and compare the average density change δ of the surface area of ​​the sample d , the average density change δ d The larger one indicates that the proportion of "dense" behavior is larger; S5: Determine the interface extension area ratio Sdr of the scratched surface of the wood material sample. A larger Sdr indicates a larger proportion of "ploughing" behavior; S6: Weigh the mass of the wood material sample again, calculate the difference with the initial mass, and divide the mass difference by the initial mass of the sample to obtain the material removal rate δ c , material removal rate δ c The larger one indicates that the "cutting" behavior accounts for a larger proportion; S7: Normalize the above evaluation values, where the interface expansion area ratio Sdr and material removal rate δ c The result is a percentage, which can be used directly as a normalized value, δ r _normalized = δ r / δ r _max, where δ r _max is the maximum tangential force value during the test, δ d _normalized = δ d / δ d _max, where δ d _max is the maximum density of the surface layer during the test. According to the requirements for the grinding results, the weights of sliding, compacting, plowing, and cutting behaviors are set to R, D, P, and C, respectively. The normalized values ​​are used to calculate the comprehensive score CS, that is, CS = (δ r _normalized*R)+(δ d _normalized*D)+(Sdr*P)+(δ c *C), a high overall score is a positive evaluation result.

2. The method according to claim 1, characterized in that In step S1, the wood material sample and the leaf-type abrasive belt strip are cut by sawing or shearing.

3. The method according to claim 1, characterized in that In step S2, a sliding scratch test device is used to perform a sliding scratch test on the wood material sample and the leaf abrasive belt strip, the wood material sample and the leaf abrasive belt strip are brought into surface contact, and the normal load, moving speed and moving distance are set.

4. The method according to claim 1, characterized in that: In step S4, the cross-sectional density is measured by X-ray cross-sectional density measurement, and in step S5, the interface extension area ratio Sdr is measured by a light section method or a laser triangulation method.

5. The sliding scratch testing device according to claim 3, characterized in that: The invention comprises a sample clamping mechanism, an abrasive belt clamping mechanism, a normal loading mechanism and a unidirectional force measuring device. The frame of the sample clamping mechanism is provided with threaded through holes, and the sample is locked with screws. The abrasive belt clamping mechanism and the normal loading mechanism are integrated. The unidirectional force measuring device comprises a spring, a mechanical sensor, a cantilever bracket and a chuck.

6. The sliding scratch testing device according to claim 5, characterized in that: The abrasive belt clamping mechanism includes a fastening screw and a belt loading area. The fastening screw is used to fasten the two ends of the leaf abrasive belt strip. The normal loading mechanism can adjust the size of the normal load by changing the mass and quantity of the added weights. The spring plays a role in accurately measuring the tangential force during the period from static to relative displacement of the wood material sample and the leaf abrasive belt strip. The cantilever bracket can be driven by a motor and move within a certain range along the horizontal slide rail inside the body, and the speed is adjustable. A cylindrical through hole is opened on the chuck.

7. The sliding scratch testing device according to claim 6, characterized in that: The abrasive belt clamping mechanism and the normal loading mechanism are integrally connected to the circular hole on the clamping head through a connecting rod and a clamping column.

8. The sliding scratch testing device according to claim 7, characterized in that: The connecting rod is connected to the clamping column via a threaded connection, and the clamping column of a suitable length can be selected according to the size change of the wood material sample in the thickness direction.