Method for evaluating insulation electrothermal aging life of high-voltage cable under stepped temperature rise condition
By using the electrothermal aging life assessment method under stepped temperature rise conditions in high-voltage cable insulation materials, combined with the Arrhenius formula, the problem of being unable to accurately evaluate the long-term life of high-voltage cable insulation materials in the existing technology is solved, and the accuracy and reliability of life assessment are achieved. performance, ensuring the safe operation of the power grid.
Patent Information
- Application Number
- CN202410732727.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to accurately evaluate the long-term service characteristics and lifespan of high-voltage cable insulation materials with existing technology. In particular, long-term withstand voltage experiments conducted at constant temperature cannot simulate temperature changes in actual working conditions, resulting in prediction results that are not in line with actual conditions.
The electrothermal aging life evaluation method of high-voltage cable insulation under step temperature rise conditions is adopted. The temperature changes in actual operation are simulated through oil bath circulation. The cumulative damage value is calculated and an electrothermal aging cumulative damage model is established based on the Arrhenius formula to evaluate the electrothermal aging life of cable insulation samples.
This method can accurately evaluate the life of high-voltage cable insulation materials while shortening the experimental time, which is closer to the actual operating conditions, improves the accuracy and reliability of the evaluation, and ensures the safe operation of the power grid.
Smart Images

Figure CN118731599A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-voltage cable insulation life assessment, and in particular to a method for assessing the electrothermal aging life of high-voltage cable insulation under step-temperature conditions. Background Art
[0002] Insulation materials for electrical equipment are an important component of the power system, and high-voltage cables are the core components of urban power grid power supply. High-voltage cable transmission has become a key means for urban power grid transformation and capacity expansion, and new energy grid connection. High-voltage cable insulation materials are mainly cross-linked polyethylene, polypropylene, ethylene propylene rubber and other insulation materials. The service characteristics of cable insulation materials largely affect the service life of high-voltage cables. Therefore, mastering the reliable insulation service characteristics of high-voltage cable insulation materials is a sufficient condition to ensure the safe operation of high-voltage cables and reliable power supply for the entire city.
[0003] At present, the research on the insulation performance of high-voltage cables at home and abroad is still at the stage of using short-time breakdown performance to characterize the characteristics of insulation materials. However, the short-time breakdown test method can only measure the short-time failure characteristics of high-voltage cable insulation, and cannot measure the long-time failure characteristics under low field strength, and it is impossible to establish an evaluation system for analyzing the long-term service characteristics of insulation materials. In order to effectively analyze the service characteristics of high-voltage cable insulation materials, it is still necessary to carry out long-time withstand voltage tests on insulation materials and analyze the "time-pressure" characteristics of breakdown. However, long-time withstand voltage tests at constant temperature often have the problem of long experimental time, and in actual operating conditions, the temperature of high-voltage cable insulation materials will change with the change of current carrying capacity in the cable, rather than being constant. Most of the current evaluation methods are the evaluation and prediction of the remaining life of the cable at a constant temperature, and do not combine the changes in the actual temperature inside the cable to predict the remaining life of the insulation material. The prediction results obtained are often not in line with the actual working conditions. Therefore, the research on high-voltage cable insulation materials needs to take into account the changes under these actual working conditions. Summary of the invention
[0004] The purpose of the present invention is to provide a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature rising conditions, which can accurately calculate the electrothermal aging life of high-voltage cable insulation samples under step-temperature rising conditions, and the life evaluation is closer to the actual operation of the high-voltage cable.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] On the one hand, the present invention provides a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions, comprising the following steps:
[0007] The high-voltage cable insulation sample and the experimental electrode are placed in an oil bath circulation beaker, and the oil bath circulation is used to simulate the step-by-step temperature increase process of the actual operation of the high-voltage cable.
[0008] According to several groups of step heating parameters, the step heating of the oil bath circulation process is controlled respectively to obtain several corresponding groups of characteristic breakdown times; the step heating parameters include the step heating starting temperature, the step heating temperature step length and the step heating temperature duration; the characteristic breakdown time is the time when the high-voltage cable insulation sample is broken down.
[0009] According to the characteristic breakdown time under different step heating parameters, the cumulative damage value under different step heating parameters is calculated; the cumulative damage value includes the cumulative damage value before breakdown and the cumulative damage value during breakdown.
[0010] Based on the cumulative damage model of high-voltage cable insulation electrothermal aging, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the cumulative damage values under different step temperature rise parameters; the cumulative damage model of high-voltage cable insulation electrothermal aging is a model established based on the Arrhenius formula according to the electric field strength and temperature step changes under the actual operating conditions of the high-voltage cable insulation.
[0011] Optionally, the cumulative damage value under a set of step temperature increase parameters is calculated according to the following formula:
[0012]
[0013] Among them, D c,l is the cumulative damage value under the step heating parameters of the first group, k is the temperature stage number at breakdown, i is the temperature stage number, exp() is the natural exponential function, B is the ratio of activation energy to the molar gas constant, T0 is the starting temperature of the step heating, Δt is the duration of the step heating, ΔT is the step heating step, Δt end is the characteristic breakdown time.
[0014] Optionally, the cumulative damage value at any temperature stage before breakdown is calculated according to the following formula:
[0015]
[0016] Among them, D ci is the cumulative damage value in the i-th temperature stage before breakdown.
[0017] The cumulative damage value in the last temperature stage before breakdown is calculated according to the following formula:
[0018]
[0019] Among them, D ck is the cumulative damage value at breakdown.
[0020] Optionally, based on the electrothermal aging cumulative damage model of high-voltage cable insulation, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the cumulative damage values under different step temperature rise parameters, specifically including the following steps:
[0021] According to the cumulative damage values under different step heating parameters, the average value of the breakdown cumulative damage is calculated.
[0022] Based on the electrothermal aging cumulative damage model of high-voltage cable insulation, the electrothermal aging life of high-voltage cable insulation samples is calculated according to the mean value of breakdown cumulative damage.
[0023] Optionally, before calculating the average breakdown cumulative damage value according to the cumulative damage values under different step temperature increase parameters, the following steps are also included:
[0024] The variance S of the cumulative damage matrix is calculated according to the following formula: 2 The ratio of activation energy to molar gas constant when (n) is at its minimum value is B:
[0025]
[0026] Among them, S 2 (n) is the dispersion of the cumulative damage matrix, D c,l is the cumulative damage value under the lth group of step heating parameters, n is the number of groups of step heating parameters, l is the group number of step heating parameters, is the mean of the cumulative damage values in the cumulative damage matrix; according to the ratio of activation energy to molar gas constant B, the cumulative damage value D under different step heating parameters is calculated c,l .
[0027] Optionally, the mean value of the breakdown cumulative damage of the high-voltage cable insulation sample is calculated according to the following formula:
[0028]
[0029] Optionally, before calculating the electrothermal aging life of the high-voltage cable insulation sample based on the electrothermal aging cumulative damage model of the high-voltage cable insulation according to the cumulative damage values under different step temperature rise parameters, the following steps are also included:
[0030] According to the electric field intensity and temperature step changes under the actual operating conditions of high-voltage cable insulation, an electrothermal aging cumulative damage model for high-voltage cable insulation is established based on the Arrhenius formula.
[0031] Optionally, the electrothermal aging cumulative damage model of high-voltage cable insulation is as follows:
[0032]
[0033] Among them, t is the electrothermal aging life of the high-voltage cable insulation sample, in years; d is the number of temperature stages within 24 hours; a is the temperature stage number; T a is the operating temperature of the ath temperature stage; exp() is the natural exponential function; Δt a is the duration of the ath temperature stage.
[0034] On the other hand, the present invention provides a system for evaluating the life of high-voltage cable insulation electro-thermal aging under step-temperature rise conditions. When the system for evaluating the life of high-voltage cable insulation electro-thermal aging under step-temperature rise conditions is run by a computer, it executes a method for evaluating the life of high-voltage cable insulation electro-thermal aging under step-temperature rise conditions as described above.
[0035] On the other hand, the present invention also provides a computer-readable storage medium having a computer program stored thereon. When the computer program is executed by a processor, the steps of the method for evaluating the electro-thermal aging life of high-voltage cable insulation under a step-temperature increase condition as described above are implemented, or the functions of the system for evaluating the electro-thermal aging life of high-voltage cable insulation under a step-temperature increase condition as described above are implemented.
[0036] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0037] The invention provides a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions. The method comprises the following steps: placing a high-voltage cable insulation sample and an experimental electrode in an oil bath circulation beaker, simulating a step-temperature increase process of actual operation of the high-voltage cable through oil bath circulation according to several groups of step-temperature increase parameters, and obtaining several groups of corresponding characteristic breakdown times; calculating cumulative damage values under different step-temperature increase parameters according to the characteristic breakdown times; establishing a high-voltage cable insulation electrothermal aging cumulative damage model based on the Arrhenius formula according to the electric field strength and temperature step changes under the actual operating conditions of the high-voltage cable insulation, and thereby calculating the electrothermal aging life of the high-voltage cable insulation sample according to the cumulative damage values under different step-temperature increase parameters. The present invention obtains the characteristic breakdown time of a high-voltage cable insulation sample under a step-temperature increase condition. On the one hand, the step-temperature increase method is used to accelerate the thermal aging of the material, which can accelerate the thermal aging of the material and reduce the aging time. The experimental time is greatly shortened while ensuring the experimental accuracy. A high-voltage cable insulation electrothermal aging cumulative damage model is established based on the Arrhenius formula. On the other hand, the electrothermal aging remaining life of the high-voltage cable insulation sample under a temperature step-temperature increase condition is calculated, and the evaluation is closer to the operating condition of the actual load change of the high-voltage cable, so that the life evaluation result of the high-voltage cable insulation sample is more accurate, which is of great significance for improving the operating reliability of the high-voltage cable and ensuring the safe operation of the power grid. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 This is a flow chart of a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions provided in Example 1 of the present invention.
[0040] Figure 2 This is a schematic diagram of the internal temperature change of high-voltage cable insulation in Example 2 of a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions provided in Example 1 of the present invention.
[0041] Figure 3 This is a structural block diagram of a system for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions provided in Example 2 of the present invention.
[0042] Figure 4 This is a diagram of the internal structure of a computer device provided in Example 4 of the present invention. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The purpose of the present invention is to provide a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions, aiming to make an accurate prediction of the remaining life of the insulation material based on the actual temperature changes inside the cable.
[0045] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0046] Example 1
[0047] like Figure 1 As shown, a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions in this embodiment includes the following steps:
[0048] S1. Place the high-voltage cable insulation sample and the experimental electrode in an oil bath circulation beaker, and simulate the step-by-step temperature increase process of the actual operation of the high-voltage cable through oil bath circulation.
[0049] S2. According to several groups of step heating parameters, the step heating of the oil bath circulation process is controlled respectively to obtain several corresponding groups of characteristic breakdown times; the step heating parameters include the step heating starting temperature, the step heating temperature step length and the step heating temperature duration; the characteristic breakdown time is the time when the high-voltage cable insulation sample is broken down.
[0050] S3. According to the characteristic breakdown time under different step heating parameters, the cumulative damage value under different step heating parameters is calculated; the cumulative damage value under a set of step heating parameters is calculated according to the following formula (1):
[0051]
[0052] Among them, D c,l is the cumulative damage value under the step heating parameters of the first group, k is the temperature stage number at breakdown, i is the temperature stage number, exp() is the natural exponential function, B is the ratio of activation energy to the molar gas constant, T0 is the starting temperature of the step heating, Δt is the duration of the step heating, ΔT is the step heating step, Δt end is the characteristic breakdown time.
[0053] Specifically, the cumulative damage value includes the cumulative damage value before breakdown and the cumulative damage value at breakdown. The cumulative damage value at any temperature stage before breakdown is calculated according to the following formula (2):
[0054]
[0055] Among them, D ci is the cumulative damage value in the i-th temperature stage before breakdown.
[0056] The cumulative damage value at breakdown is calculated according to the following formula (3):
[0057]
[0058] Among them, D ck is the cumulative damage value at breakdown.
[0059] S4. Based on the cumulative damage model of high-voltage cable insulation electrothermal aging, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the cumulative damage values under different step temperature rise parameters. Before step S4, the following steps need to be performed:
[0060] According to the electric field strength and temperature step changes under the actual operating conditions of high-voltage cable insulation, the electric-thermal aging cumulative damage model of high-voltage cable insulation is established based on the Arrhenius formula. Specifically, it includes the following steps:
[0061] For any set of step heating parameters, several step heating experiments in the oil bath cycle process were carried out to obtain several cumulative damage values under the step heating parameters.
[0062] According to several cumulative damage values obtained from each group of step heating parameters, a cumulative damage matrix is determined.
[0063] The optimal ratio of activation energy to molar gas constant is determined based on minimizing the dispersion of the cumulative damage matrix.
[0064] Based on the Arrhenius formula, a cumulative damage model of high-voltage cable insulation electrothermal aging was established according to the optimal ratio of activation energy to molar gas constant.
[0065] The following is a further description of the process of constructing the high-voltage cable insulation electrothermal aging cumulative damage model based on the Arrhenius formula:
[0066] The Arrhenius life formula is shown in equation (4):
[0067]
[0068] Among them, M is a characteristic aging value of cable insulation, A is the Arrhenius constant, E i is the experimental activation energy, which can generally be considered as a constant independent of temperature, with the unit of J / mol; T is the absolute temperature, with the unit of K; R is the molar gas constant, with the unit of J·mol -1 ·K -1 ; t represents the remaining life of the material at this temperature. For ease of expression, the Arrhenius life formula is simplified to the following form (5):
[0069]
[0070] Among them, D c,l is the cumulative damage area of the material, B represents the activation energy E i The ratio of the molar gas constant R, that is, E i / R.
[0071] Therefore, the damage caused to the insulating material sample at any temperature stage in the step temperature rise experiment can be calculated according to the following formula (6):
[0072]
[0073] The cumulative damage caused in the last temperature stage is calculated by the following formula (7):
[0074]
[0075] Then, during the entire step-up heating process of the first group of step-up heating parameters, the cumulative damage caused is calculated by the following formula (8):
[0076]
[0077] Set n groups of step temperature rise parameters (T0, ΔT, Δt), and repeat each group of step temperature rise experiments m times to ensure the accuracy of the experimental results under AC voltage. Obtain the characteristic breakdown time of high-voltage cable insulation under m groups of step temperature rise conditions, and take the average value of m characteristic breakdown times as the characteristic breakdown time of this group of step temperature rise parameters.
[0078] According to a basic assumption of the step temperature rise experiment: the cumulative damage required to cause the breakdown of XLPE material is a constant D c,l , D c,l The value of has nothing to do with the accumulation mode of cumulative damage, that is, it has nothing to do with the heating mode. Therefore, the most suitable fitting parameter B is found to make the values of each element in the cumulative damage matrix D closer and the dispersion smaller. It is believed that the fitting parameter B is the true value of the unknown parameter B of the XLPE material under experimental conditions. c,l The variance S 2 Characterize the dispersion of D, the calculation formula is shown in the following formula (9):
[0079]
[0080] Among them, S 2 (n) is the dispersion of the cumulative damage matrix, D c,l is the cumulative damage value under the lth group of step heating parameters, n is the number of groups of step heating parameters, l is the group number of step heating parameters, is the mean of the cumulative damage values in the cumulative damage matrix, that is, the mean of the breakdown cumulative damage of the high-voltage cable insulation sample. According to the ratio B of the activation energy to the molar gas constant, the cumulative damage value D under different step temperature rise parameters is calculated. c,l .
[0081] Step S4 specifically includes the following steps:
[0082] S41. Calculate the mean value of the cumulative damage under different step temperature rise parameters. Substitute the parameter B calculated above into the cumulative damage model of high-voltage cable insulation electrothermal aging to obtain the cumulative damage required for the breakdown of each group of insulation material samples in the step temperature rise experiment. Due to the traditional factors such as the XLPE sample preparation process, inherent defects in the XLPE sample, step temperature rise experiment operation errors, system errors, environmental factors, etc., the cumulative damage may have a certain dispersion. The cumulative damage mean of multiple groups of repeated experiments under each group of step temperature rise parameters in the cumulative damage matrix is obtained as the cumulative damage under this group of step temperature rise parameters; the mean value of the cumulative damage under the breakdown is calculated according to the following formula (10):
[0083]
[0084] in, is the mean value of the breakdown cumulative damage, D c,l is the cumulative damage value under the lth group of step heating parameters, n is the number of groups of step heating parameters, and l is the group number of step heating parameters.
[0085] S42. Based on the cumulative damage model of high-voltage cable insulation electrothermal aging, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the mean value of the breakdown cumulative damage. The cumulative damage model of high-voltage cable insulation electrothermal aging is shown in the following formula (11):
[0086]
[0087] Where t is the electrothermal aging life of the high-voltage cable insulation sample (in years), d is the number of temperature stages within 24 hours, a is the temperature stage number, T a is the working temperature of the ath temperature stage, exp() is the natural exponential function, that is, the exponential function with the real number e (e≈2.71828) as the base, B is the ratio of activation energy to the molar gas constant, Δt a is the duration of the ath temperature stage.
[0088] The following two examples are used to specifically illustrate the method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions provided in this embodiment.
[0089] Example 1:
[0090] Step A1: Place the high-voltage cable insulation flat plate vulcanization sample and the experimental electrode in an oil bath circulation beaker, and simulate the step temperature rise process of the actual operation of the cable through oil bath circulation.
[0091] Step A2: Set the starting temperature T0, the temperature step length ΔT and the duration Δt of each temperature for three sets of step temperature rise tests. The parameters of the three sets of step temperature rise tests are as follows:
[0092] Ⅰ: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 200s, and the heating step ΔT is 5℃.
[0093] Ⅱ: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 300s, and the heating step ΔT is 5℃.
[0094] III: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 500s, and the heating step ΔT is 5℃.
[0095] During the step-by-step temperature increase process, a constant electric field is applied to the vulcanized sample of the high-voltage cable insulation flat plate. In this embodiment, the constant field strength is selected as 40% of the short-time breakdown field strength, that is, 40 kV / mm.
[0096] Step A3: Obtain characteristic breakdown time of high-voltage cable insulation samples under three groups of different step temperature rise parameters (T0, ΔT, Δt), and calculate the cumulative damage value D of each group through the characteristic breakdown time of high-voltage cable insulation samples under different step temperature rise parameters (T0, ΔT, Δt). c,l ;
[0097] Three groups of step-heating parameters, Ⅰ, Ⅱ, and Ⅲ, were used to test 10 groups of samples each. The experimental data caused by experimental errors or acquisition equipment were eliminated, and the average value of the ten groups of data was calculated. The following data was obtained:
[0098] Group Breakdown time(s) Final breakdown temperature(℃) Ⅰ 3560 115 Ⅱ 3840 90 Ⅲ 4450 70
[0099] Calculate the cumulative damage of the three groups I, II, and III, and substitute the parameters into formula (8). The calculation results are as follows:
[0100]
[0101] Among them, 160, 240 and 450 represent the breakdown time t end ; 303 represents the starting temperature T0 of the step temperature rise at Kelvin temperature; 17, 12 and 8 represent the final breakdown temperature after 17, 12 and 8 ΔT respectively. At this time, even if B is the same, there will be three different cumulative damages D c,l According to a basic assumption of the step temperature rise experiment, the cumulative damage required to cause the breakdown of XLPE material is a constant D c,l , D c,l The value of has nothing to do with the accumulation mode of cumulative damage, that is, it has nothing to do with the heating mode. Therefore, the most suitable fitting parameter B is found to make the values of each element in the cumulative damage matrix D closer and the dispersion smaller. It is believed that this fitting parameter is the true value of the unknown parameter B of the XLPE material under experimental conditions. c,l The variance S 2 Characterize the dispersion of D. Use Newton iteration method to calculate the most suitable fitting parameter B to minimize the variance.
[0102] The calculation results are as follows:
[0103] Under the optimal parameters D c,l The result is: D in Scheme I c,1 The calculated value is 3.82×10 5 ; Scheme II D c,2 The calculated value is: 4.12×10 5 ; D in Scheme III c,3 The calculated value is: 3.76×10 5 , at this time B is 2178.
[0104] At this time, under the three options D c,l The average value of
[0105]
[0106] Step A4: In this example, the case where the cable insulation temperature is constant under the actual operating conditions of the high-voltage cable is considered, and an electrothermal aging cumulative damage model of the insulation sample is established based on the Arrhenius formula to calculate the electrothermal aging life of the high-voltage cable insulation.
[0107]
[0108] Wherein, t represents the remaining life of the material in years. For example, the remaining life of the material at 50°C is 10.48 years.
[0109] Example 2:
[0110] Step B1, placing the high-voltage cable insulation cable cut sample and the experimental electrode in an oil bath circulation beaker, and simulating the step-by-step heating process of the actual operation of the cable through oil bath circulation;
[0111] Step B2, set the starting temperature T0, the temperature step length ΔT and the duration Δt of each temperature for three sets of step temperature rise tests. The parameters of the three sets of step temperature rise tests are as follows:
[0112] IV: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 400s, and the heating step ΔT is 5℃.
[0113] Ⅴ: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 500s, and the heating step ΔT is 5℃.
[0114] VI: The initial temperature T0 of heating is 30℃, the heating time interval Δt is 600s, and the heating step ΔT is 5℃.
[0115] During the step-by-step heating process, a constant electric field is applied to the high-voltage cable insulation coiled sample. In this embodiment, the constant field strength is selected as 50% of the short-time breakdown field strength, that is, 50 kV / mm.
[0116] Step B3, obtain the characteristic breakdown time of high-voltage cable insulation samples under three different step temperature parameters (T0, ΔT, Δt), and calculate the cumulative damage value D of each group through the characteristic breakdown time of high-voltage cable insulation samples under different step temperature parameters (T0, ΔT, Δt). c,l ;
[0117] There are three schemes: IV, V, and VI. Each scheme tests 10 groups of samples. The experimental data caused by experimental errors or acquisition equipment are eliminated, and the average value of the ten groups of data is calculated. The following data is obtained:
[0118] Group Breakdown time(s) Final breakdown temperature(℃) Ⅳ 6650 110 Ⅴ 6350 90 Ⅵ 7060 85
[0119] Calculate the cumulative damage of the three groups IV, V, and VI, and substitute the parameters into formula (8). The calculation results are as follows:
[0120]
[0121] 250, 350 and 460 represent the breakdown time t end ; 303 represents the starting temperature T0 of the step heating at Kelvin temperature; 16, 12 and 11 represent the final breakdown temperature after 16, 12 and 11 ΔT respectively. Next, the Newton iteration method is used to calculate the most suitable fitting parameter B so that the variance S 2 Minimum.
[0122] The calculation results are as follows:
[0123] Under the optimal parameters D c,l The result is: D in Scheme IV c,1 The calculated value is 4.12×10 6 ; Scheme V D c,2 The calculated value is: 3.25×10 6 ; D in Scheme VI c,3 The calculated value is: 4.52×10 6 . At this time, B is 1972.
[0124] At this time, under the three options D c,l The average value of
[0125]
[0126] Step B4: In this embodiment, the step-like change of cable insulation temperature under actual operating conditions of the high-voltage cable is considered, and an electrothermal aging cumulative damage model of the insulation sample is established based on the Arrhenius formula to calculate the electrothermal aging life of the high-voltage cable insulation.
[0127] Figure 2 The internal temperature of high-voltage cable insulation varies with daily load. Figure 2 The situation further explains the calculation of the remaining life of the material. Within 24 hours, the internal temperature of the high-voltage cable insulation experienced five stages of change, 2:00-7:00, 7:00-13:00, 13:00-18:00, 18:00-22:00, 22:00-2:00, and the corresponding step temperature change parameters (T a , Δt a ) are (303K, 5h), (363K, 6h), (343K, 5h), (363K, 4h), (313K, 4h) respectively. The remaining life of the high voltage cable insulation material in this case is calculated as:
[0128]
[0129] Where t represents the remaining life of the material in years. a Δt is the step temperature corresponding to different time periods of high-voltage cable insulation within 24 hours, in K; a It indicates the duration of different step temperatures within the 24 hours, in seconds; d indicates the number of temperature stages within every 24 hours.
[0130] The present embodiment provides a method for evaluating the life of high-voltage cable insulation under step-temperature conditions. The characteristic breakdown time of the high-voltage cable insulation sample is obtained under step-temperature conditions. The thermal aging of the material is accelerated by the step-temperature method, which can accelerate the thermal aging of the material and reduce the aging time. The experimental time is greatly shortened while ensuring the accuracy of the experiment. A cumulative damage model for the electric thermal aging of the high-voltage cable insulation is established based on the Arrhenius formula, and the remaining life of the electric thermal aging of the high-voltage cable insulation under the condition of temperature step-temperature changes is calculated. The evaluation is closer to the actual operation of the high-voltage cable, thereby making the evaluation result more accurate, which is of great significance for improving the operating reliability of the high-voltage cable and ensuring the safe operation of the power grid.
[0131] Example 2
[0132] In addition, the method for evaluating the electrothermal aging life of high-voltage cable insulation under step-by-step temperature rise conditions in Example 1 of the present invention can also be used to Figure 3 The structure of the high-voltage cable insulation electrothermal aging life evaluation system under step-by-step temperature rise conditions is shown in FIG. Figure 3 As shown, the high-voltage cable insulation electrothermal aging life assessment system under the step temperature rise condition may include an oil bath cycle simulation module M1, a step temperature rise parameter generation module M2, a step temperature rise simulation module M3, a characteristic breakdown time recording module M4, a cumulative damage value calculation module M5 and an electrothermal aging life calculation module M6; some modules may also have sub-units for realizing their functions. Of course, Figure 3The architecture shown is only exemplary and can be omitted according to actual needs when implementing different functions. Figure 3 One or at least two components of the system shown.
[0133] Example 3
[0134] A computer-readable storage medium stores a computer program, which, when executed by a processor, implements the steps of a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions in Example 1.
[0135] Example 4
[0136] This embodiment provides a computer device, which can be a database, and its internal structure diagram can be as follows: Figure 4 As shown. The computer device includes a processor, a memory, an input / output interface (Input / Output, referred to as I / O) and a communication interface. Among them, the processor, the memory and the input / output interface are connected through a system bus, and the communication interface is connected to the system bus through the input / output interface. Among them, the processor of the computer device is used to provide computing and control capabilities. The memory of the computer device includes a non-volatile storage medium and an internal memory. The non-volatile storage medium stores an operating system, a computer program and a database. The internal memory provides an environment for the operation of the operating system and the computer program in the non-volatile storage medium. The database of the computer device is used to store pending transactions. The input / output interface of the computer device is used to exchange information between the processor and an external device. The communication interface of the computer device is used to communicate with an external terminal through a network connection. When the computer program is executed by the processor, the steps of a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-by-step temperature rise conditions in Example 1 are implemented.
[0137] It should be noted that the object information (including but not limited to object device information, object personal information, etc.) and data (including but not limited to data used for analysis, stored data, displayed data, etc.) involved in the present invention are all information and data authorized by the object or fully authorized by all parties, and the collection, use and processing of relevant data need to comply with relevant laws, regulations and standards of relevant countries and regions.
[0138] Those skilled in the art can understand that all or part of the processes in the above-mentioned embodiments can be completed by instructing the relevant hardware through a computer program, and the computer program can be stored in a non-volatile computer-readable storage medium. When the computer program is executed, it can include the processes of the embodiments of the above-mentioned methods. Among them, any reference to the memory, database or other medium used in the embodiments provided by the present invention can include at least one of non-volatile and volatile memory. Non-volatile memory can include read-only memory (ROM), magnetic tape, floppy disk, flash memory, optical memory, high-density embedded non-volatile memory, resistive random access memory (ReRAM), magnetoresistive random access memory (MRAM), ferroelectric random access memory (FRAM), phase change memory (PCM), graphene memory, etc. Volatile memory can include random access memory (RAM) or external cache memory, etc. As an illustration and not limitation, RAM can be in various forms, such as static random access memory (SRAM) or dynamic random access memory (DRAM). The database involved in each embodiment provided by the present invention may include at least one of a relational database and a non-relational database. Non-relational databases may include distributed databases based on blockchains, etc., but are not limited thereto. The processor involved in each embodiment provided by the present invention may be a general-purpose processor, a central processing unit, a graphics processor, a digital signal processor, a programmable logic device, a data processing logic device based on quantum computing, etc., but are not limited thereto.
[0139] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0140] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions, characterized in that: include: The high-voltage cable insulation sample and the experimental electrode are placed in an oil bath circulation beaker, and the oil bath circulation is used to simulate the step-by-step temperature increase process of the actual operation of the high-voltage cable; According to several groups of step heating parameters, the step heating of the oil bath circulation process is controlled respectively to obtain several groups of corresponding characteristic breakdown times; the step heating parameters include the step heating starting temperature, the step heating temperature step length and the step heating temperature duration; the characteristic breakdown time is the time when the high-voltage cable insulation sample is broken down; According to the characteristic breakdown time under different step heating parameters, the cumulative damage value under different step heating parameters is calculated; the cumulative damage value includes the cumulative damage value before the breakdown and the cumulative damage value during the breakdown; Based on the cumulative damage model of high-voltage cable insulation electrothermal aging, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the cumulative damage values under different step temperature rise parameters; the cumulative damage model of high-voltage cable insulation electrothermal aging is a model established based on the Arrhenius formula according to the electric field strength and temperature step changes under the actual operating conditions of the high-voltage cable insulation.
2. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 1 is characterized in that: The cumulative damage value under a set of step temperature increase parameters is calculated according to the following formula: Among them, D c,l is the cumulative damage value under the step heating parameters of the first group, k is the temperature stage number at breakdown, i is the temperature stage number, exp() is the natural exponential function, B is the ratio of activation energy to the molar gas constant, T0 is the starting temperature of the step heating, Δt is the duration of the step heating, ΔT is the step heating step, Δt end is the characteristic breakdown time.
3. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 2 is characterized in that: The cumulative damage value at any temperature stage before breakdown is calculated according to the following formula: Among them, D ci is the cumulative damage value of the i-th temperature stage before breakdown; The cumulative damage value in the last temperature stage before breakdown is calculated according to the following formula: Among them, D ck is the cumulative damage value at breakdown.
4. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 1 is characterized in that: Based on the cumulative damage model of high-voltage cable insulation electrothermal aging, the electrothermal aging life of high-voltage cable insulation samples is calculated according to the cumulative damage values under different step temperature rise parameters, including: According to the cumulative damage values under different step temperature rise parameters, the average value of the breakdown cumulative damage is calculated; Based on the electrothermal aging cumulative damage model of high-voltage cable insulation, the electrothermal aging life of the high-voltage cable insulation sample is calculated according to the breakdown cumulative damage mean.
5. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 4 is characterized in that: Before calculating the average breakdown cumulative damage value based on the cumulative damage values under different step temperature rise parameters, it also includes: The variance S of the cumulative damage matrix is calculated according to the following formula: 2 The ratio of activation energy to molar gas constant when (n) is at its minimum value is B: Among them, S 2 (n) is the dispersion of the cumulative damage matrix, D c,l is the cumulative damage value under the lth group of step heating parameters, n is the number of groups of step heating parameters, l is the group number of step heating parameters, is the mean of the cumulative damage values in the cumulative damage matrix; according to the ratio of activation energy to molar gas constant B, the cumulative damage value D under different step heating parameters is calculated c,l .
6. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 5 is characterized in that: The mean value of the breakdown cumulative damage of the high-voltage cable insulation sample is calculated according to the following formula:
7. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 6 is characterized in that: Before calculating the electrothermal aging life of high-voltage cable insulation samples based on the electrothermal aging cumulative damage model of high-voltage cable insulation and the cumulative damage values under different step temperature rise parameters, it also includes: According to the electric field intensity and temperature step changes under the actual operating conditions of high-voltage cable insulation, an electrothermal aging cumulative damage model for high-voltage cable insulation is established based on the Arrhenius formula.
8. The method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions according to claim 7 is characterized in that: The electrothermal aging cumulative damage model of high-voltage cable insulation is shown in the following formula: Among them, t is the electrothermal aging life of the high-voltage cable insulation sample, in years; d is the number of temperature stages within 24 hours; a is the temperature stage number; T a is the operating temperature of the ath temperature stage; exp() is the natural exponential function; Δt a is the duration of the ath temperature stage.
9. A system for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature conditions, characterized in that: The system for evaluating the life of high-voltage cable insulation under step-temperature rise conditions for electrothermal aging is executed by a computer to execute a method for evaluating the life of high-voltage cable insulation under step-temperature rise conditions for electrothermal aging as described in any one of claims 1 to 8.
10. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the computer program is executed by a processor, the steps of a method for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature rise conditions described in any one of claims 1 to 8 are implemented, or the functions of a system for evaluating the electrothermal aging life of high-voltage cable insulation under step-temperature rise conditions described in claim 9 are implemented.
Citation Information
Cited By
Crosslinked polyethylene cable insulation aging risk assessment method
CN119716414A