A high brightness scratch-resistant coated reflective film and preparation method thereof

By using a high hydroxyl content acrylic resin adhesive and large-particle PU particles in the reflective film combined with polymethyl methacrylate to coat TiO2 particles, the scratching of the reflective film and the light guide plate during the coating treatment is solved. The problem of top whitening improves the scratch resistance, top whitening resistance and brightness of the reflective film, and improves the display effect of the monitor.

CN118732107BActive Publication Date: 2024-11-19NINGBO CHANGYANG TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411233917.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-19
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The existing reflective films are prone to scratches or whitening defects in the light guide plate during the coating process, and the brightness is insufficient, affecting the visual experience of the display.

Method used

A high-bright scratch-resistant reflective film including a UV adhesive layer, a reflective base film and a coating layer is used. The coating layer is composed of an adhesive layer and a composite particle, and the composite particles are coated with polyurethane particles and polymethyl methacrylate. TiO2 particles, the adhesive layer consists of acrylic resin adhesive with high hydroxyl content and large-particle PU particles, and the UV adhesive layer provides support on the back of the reflective film.

Benefits of technology

It significantly improves the scratch resistance, anti-top whiteness and brightness of the reflective film, avoids scratching of the light guide plate, enhances the overall performance of the backlight module, and provides a higher quality display effect for the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732107B_ABST
    Figure CN118732107B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of optical reflective films, and relates to a high-brightness scratch-resistant coated reflective film and a preparation method thereof. The reflective film comprises a UV adhesive layer, a reflective base film and a coating layer in sequence, the coating layer comprises an adhesive layer and composite particles, the adhesive layer is bonded to the surface of the reflective base film, and the composite particles are distributed in the adhesive layer; the composite particles comprise PU particles and PMMA-coated TiO2 particles; the average particle size of the polyurethane particles is 10-30 μm, and the average particle size of the polymethyl methacrylate-coated TiO2 particles is 1-8 μm; the mass ratio of the polyurethane particles to the polymethyl methacrylate-coated TiO2 particles is 1:70-120. The reflective film provided by the present invention has high brightness and excellent scratch resistance and anti-whitening performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical reflective films and relates to a high-brightness scratch-resistant coated reflective film and a preparation method thereof. Background Art

[0002] As one of the key components of the display, the backlight module contains a variety of optical films, such as diffusion films, brightness enhancement films and reflective films. These components work together to ensure that the backlight module can provide light evenly and efficiently, thereby improving the display effect. The backlight module can be roughly divided into two types: edge-type and direct-type according to the position of the light source. In the edge-type backlight module, the light guide plate converts the point light source into a surface light source, and the reflective film is located on the back of the light guide plate to improve light utilization, reduce light loss, and ensure a more uniform backlight.

[0003] If the reflective film is not coated, adsorption problems will occur, resulting in appearance defects such as dark shadows, so it is generally coated; however, the selection of coating particles is crucial to the performance of the reflective film. If the coated particles are too hard, they may scratch the light guide plate during the assembly of the backlight module, resulting in defects such as linear scratches after the backlight module is lit; if the coated particles are too soft, the backlight module will also have white top defects after lighting due to excessive local pressure during transportation. Coated particles are generally polymer materials, which will swell in solvents: due to the large difference in size between solvent molecules and polymers, the molecular movement speed is also different, and the solvent molecules diffuse faster than the polymer diffuses into the solvent. The solvent molecules will penetrate into the polymer material, increasing its volume. Particles with increased volume are easy to break through the glue layer, and there is a risk of scratching the light guide plate. If the adhesive layer is too thin, it may not be able to fix larger particles, causing them to fall off during the production process. Although a thicker adhesive layer can prevent large particles from falling off, it will reduce the brightness of the coated reflective film, and the reduced brightness will reduce the overall visual experience of the display. Therefore, scratch resistance, anti-whitening, and high brightness have become important indicators for measuring the performance of coated reflective films. Summary of the invention

[0004] In order to further improve the performance of the reflective film, the present invention proposes a coated reflective film and a preparation method thereof, aiming to improve the brightness and anti-scratch and anti-whitening performance of the reflective film. It not only solves the existing technical problems, but also significantly improves the overall performance of the backlight module, providing a higher quality display effect for the display device.

[0005] One object of the present invention is achieved by the following technical solutions:

[0006] A high-brightness scratch-resistant coated reflective film, comprising a UV adhesive layer, a reflective base film and a coating layer in sequence, wherein the coating layer comprises an adhesive layer and composite particles, wherein the adhesive layer is bonded to the surface of the reflective base film, and the composite particles are distributed in the adhesive layer;

[0007] The composite particles include polyurethane (PU) particles and polymethyl methacrylate (PMMA)-coated TiO2 particles;

[0008] The average particle size of polyurethane particles is 10~30μm, and the average particle size of polymethyl methacrylate coated TiO2 particles is 1~8μm;

[0009] The mass ratio of polyurethane particles to polymethyl methacrylate coated TiO2 particles is 1:70~120.

[0010] Preferably, the average particle size of the polyurethane particles is 12-17 μm, and the average particle size of the polymethyl methacrylate-coated TiO2 particles is 3-5 μm.

[0011] Preferably, the mass ratio of polyurethane particles to polymethyl methacrylate coated TiO2 particles is 1:80 to 110. It can be 1:80, 1:85, 1:90, 1:95, 1:100, 1:105 or 1:110, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0012] Preferably, the method for preparing the polymethyl methacrylate coated TiO2 particles comprises the following steps:

[0013] The TiO2 particles are dispersed in an acid solution for pretreatment;

[0014] The pretreated TiO2 particles are dispersed in an organic solvent, and then acetic acid and azobisisobutyronitrile are added. When the temperature rises to 50-80°C, methyl methacrylate is added to react.

[0015] After the reaction is completed, the product is washed and centrifuged to obtain polymethyl methacrylate-coated TiO2 particles.

[0016] In the preparation process of the PMMA-coated TiO2 particles, the acid solution is not particularly limited and can be a hydrochloric acid solution, a sulfuric acid solution, a nitric acid solution, an acetic acid solution, etc. The organic solvent can be methanol, ethanol, acetone, etc. Preferably, the pH of the acid solution is 1 to 3. Preferably, the volume of the acid solution and the mass ratio of the TiO2 particles are 5 to 500 ml: 1 g. Preferably, the mass ratio of the organic solvent: TiO2: acetic acid: methyl methacrylate: azobisisobutyronitrile is 240: (1.5 to 15): (0.5 to 5): (5 to 50): (0.2 to 3). Preferably, methyl methacrylate is added to react for 5 to 30 hours. After the reaction is completed, it is washed several times with methanol, ethanol, etc., and then centrifuged at 1000 to 5000 r / min for 10 to 50 minutes.

[0017] Preferably, the TiO2 particles are hollow TiO2 particles, that is, the polymethyl methacrylate-coated TiO2 particles are polymethyl methacrylate-coated hollow TiO2 particles.

[0018] Preferably, the coating layer is prepared from a coating liquid, wherein the coating liquid comprises: 20 to 40 parts of an adhesive, 10 to 30 parts of composite particles, 35 to 55 parts of a solvent, and 1 to 5 parts of a curing agent.

[0019] Preferably, the coating liquid is coated on one side of the reflective base film and cured to obtain a coating layer.

[0020] More preferably, the coating solution also includes 0.1 to 1 part of an antistatic agent.

[0021] Preferably, the adhesive is an acrylic resin adhesive.

[0022] More preferably, the solid content of the acrylic resin adhesive is 25-85wt%.

[0023] More preferably, the acrylic resin adhesive has a hydroxyl content of 20-40 mg KOH / g (solid). Each gram of solid acrylic resin contains 20 to 40 mg of hydroxyl (-OH) functional groups equivalent to potassium hydroxide.

[0024] Preferably, the solvent is one or more of ethyl acetate, butyl acetate and butanone.

[0025] More preferably, the solvent is a mixture of ethyl acetate and butyl acetate in a volume ratio of 1:0.2-5.

[0026] Preferably, the curing agent is an aliphatic polyisocyanate, which may be hexamethylene diisocyanate (HDI) based polyisocyanate, isophorone diisocyanate (IPDI) based polyisocyanate, tetramethylxylylene diisocyanate (TMXDI) based polyisocyanate, cyclohexane diisocyanate (CHDI) based polyisocyanate, or the like.

[0027] Preferably, the antistatic agent is a quaternary ammonium salt antistatic agent, which can be exemplified by dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, and the like.

[0028] Preferably, the UV adhesive layer is prepared from UV slurry, and the UV slurry includes: 30-45 parts of solvent, 1-5 parts of photocuring agent and 50-70 parts of photosensitive resin adhesive.

[0029] Preferably, in the UV slurry, the solvent is one or more of ethyl acetate, butyl acetate and butanone.

[0030] Preferably, in the UV slurry, the photocuring agent is aliphatic polyisocyanate.

[0031] Preferably, in the UV slurry, the photosensitive resin adhesive is trifunctional polyurethane acrylate, and the solid content is 25-65wt%.

[0032] Preferably, the UV slurry is coated on the other side of the reflective base film, and a UV adhesive layer is obtained after pre-curing and UV curing.

[0033] Another object of the present invention is achieved by the following technical solutions:

[0034] A method for preparing a high-brightness scratch-resistant coated reflective film comprises the following steps:

[0035] Add the raw materials in the coating liquid into the liquid preparation tank, stir for 5 to 300 minutes to form the coating liquid, apply the coating liquid on one side of the reflective base film, obtain the coating layer after curing, and then ripen;

[0036] The raw materials of UV slurry are added into a liquid preparation tank and stirred for 5 to 300 minutes to form UV slurry. The UV slurry is coated on the other side of the matured reflective base film. After pre-curing and UV curing, a UV adhesive layer is obtained, that is, the high-brightness scratch-resistant coated reflective film is obtained.

[0037] Preferably, the coating liquid is coated on one side of the reflective base film to a thickness of 10 to 15 μm.

[0038] Preferably, the curing temperature of the coating liquid is 100-120° C., and the curing time is 1-5 min.

[0039] Preferably, the aging temperature is 50-70° C. and the aging time is 10-30 hours.

[0040] Preferably, the thickness of the UV slurry coated on the other side of the aged reflective base film is 1-5 μm.

[0041] Preferably, the pre-curing temperature of the UV slurry is 70-90° C., and the pre-curing time is 0.5-4 min.

[0042] Preferably, the UV energy of UV curing is 200-800 mJ / cm 2 .

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] (1) The reflective film of the present invention comprises a coating layer, which comprises an adhesive, large-diameter polyurethane particles and small-diameter PMMA-coated TiO2 particles. The adhesive is an acrylic resin adhesive with a high hydroxyl content, so that the adhesive layer is rigid and can effectively bind large and small particles inside the adhesive layer, thereby preventing large and small particles from breaking through the adhesive layer and scratching the light guide plate, thereby showing good anti-scratch performance; the large-diameter PU particles play a supporting role when the light guide plate is subjected to pressure, so that the coated reflective film has good anti-whitening performance, and PU is a relatively soft polymer material, which can also avoid scratching the light guide plate; the use of polymethyl methacrylate to coat titanium dioxide can improve the reflectivity of the coated reflective film to a certain extent, increase the utilization rate of light, and thus improve the brightness.

[0045] (2) The reflective film of the present invention further comprises a UV adhesive layer, which is coated on the back of the reflective film. The UV adhesive layer plays a supporting role and improves the anti-whitening effect of the reflective film.

[0046] (3) The mass ratio of the large-size PU particles to the small-size PMMA-coated TiO2 particles of the present invention is 1:70-120. A small amount of PU particles is not conducive to improving the anti-whitening effect, while a large amount of PU particles will result in an insignificant improvement in reflectivity.

[0047] (4) The present invention further prefers PMMA-coated hollow TiO2, and the incident light is scattered multiple times on the outer surface and inner surface of the hollow titanium dioxide, thereby obtaining a higher reflectivity; in addition, the effect of PMMA-coated hollow TiO2 on improving the reflectivity is significantly better than that of PMMA-coated non-hollow TiO2. After the hollow TiO2 is coated with PMMA, the reflectivity is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a schematic structural diagram of the reflective film provided by the present invention.

[0049] Among them, 1. PMMA coated TiO2 particles, 2. PU particles, 3. adhesive layer, 4. reflective base film, 5. UV adhesive layer. DETAILED DESCRIPTION

[0050] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0051] Figure 1The structure diagram of the reflective film provided by the present invention is shown in FIG. Figure 1 It can be seen that the reflective film of the present invention comprises a UV adhesive layer 5, a reflective base film 4 and a coating layer in sequence, the coating layer comprises an adhesive layer 3 and composite particles, the adhesive layer 3 is bonded to one side of the reflective base film 4, the UV adhesive layer 5 is bonded to the other side of the reflective base film 4, and the composite particles are distributed in the adhesive layer 3; the composite particles comprise PU particles 2 and PMMA-coated TiO2 particles 1.

[0052] In the following examples and comparative examples, the sources of the raw materials are as follows:

[0053] The curing agent and light curing agent are both HDI-based polyisocyanate, model PB98242, provided by Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0054] The reflective base film is the EST150 reflective film made by the applicant;

[0055] The photosensitive resin adhesive is trifunctional polyurethane acrylate with a solid content of 30 wt %, provided by Edison Company, model U-CURE 9320.

[0056] PMMA coated TiO2 particles were prepared by the following preparation method:

[0057] 9g of non-hollow TiO2 particles were dispersed in 100ml of hydrochloric acid solution with a pH of 1 and stirred for pretreatment for 50min, and the pretreated TiO2 particles were filtered and then dispersed in 720g of methanol, and then 3g of acetic acid and 1.8g of azobisisobutyronitrile were added. When the temperature was raised to 65°C, 36g of methyl methacrylate was added to react for 15h; after the reaction, the product was washed with methanol and centrifuged at 3000r / min for 30min to obtain powdered PMMA-coated TiO2 particles. The average particle size of PMMA-coated TiO2 particles was 4μm.

[0058] The hollow TiO2 particles are prepared by the following preparation method:

[0059] Raw materials: anhydrous ethanol, polystyrene (3.7~4μm), tetrabutyl titanate, ammonia water.

[0060] Preparation method: 2.5g polystyrene is dispersed in 100mL anhydrous ethanol and ultrasonically treated for 30min; 5mL tetrabutyl titanate is added to the mixed solution and stirred evenly; 5mL ammonia water is added to the mixed solution at room temperature and stirred for 10h; the obtained mixed solution is centrifuged to obtain titanium dioxide-coated styrene microspheres. Finally, the product is calcined at 650~700℃ for 3h and cooled to room temperature to obtain hollow TiO2 microspheres.

[0061] The preparation method of PMMA coated hollow TiO2 particles is the same as PMMA coated TiO2 particles, and the above hollow TiO2 particles are substituted for non-hollow TiO2 particles. The average particle size of PMMA coated hollow TiO2 particles is 4 μm. Example 1

[0062] The coating liquid raw materials include: 30 parts of acrylic resin adhesive (hydroxyl value content is 33 mgKOH / g (solid), solid content is 65wt%), 0.2 parts of PU particles (average particle size is 17μm), 19.8 parts of PMMA coated TiO2, 46.5 parts of ethyl acetate and butyl acetate with a volume ratio of 1:1, 0.5 parts of dodecyltrimethylammonium chloride antistatic agent, and 3 parts of HDI-based polyisocyanate.

[0063] The raw materials of UV slurry include: 60 parts of photosensitive resin adhesive, 37 parts of ethyl acetate, and 3 parts of light curing agent.

[0064] The reflective film preparation method of this embodiment comprises the following steps: adding the raw materials in the coating liquid into a liquid preparation tank, stirring at 1000 rpm for 60 min to form a coating liquid, coating the coating liquid on one side of the reflective base film with a coating thickness of 15 μm, curing at 120° C. for 2 min, and finally aging at 60° C. for 20 h; adding the raw materials of the UV slurry into a liquid preparation tank, stirring at 1000 rpm for 60 min to form a UV slurry, coating the UV slurry on the other side of the aged reflective base film with a coating thickness of 3 μm, curing at 85° C. for 2 min, and then passing through a UV curing machine, with the UV energy controlled at 400 mJ / cm 2 , and the speed is 3.6 m / min to obtain a UV adhesive layer, that is, the reflective film of this embodiment. Example 2

[0065] The coating liquid raw materials include: 25 parts of acrylic resin adhesive (hydroxyl value content is 33 mgKOH / g (solid), solid content is 65wt%), 0.2 parts of PU particles (average particle size is 17μm), 14.8 parts of PMMA coated TiO2, 40 parts of ethyl acetate and butyl acetate with a volume ratio of 1:1, 0.3 parts of tetradecyltrimethylammonium chloride antistatic agent, and 2 parts of HDI-based polyisocyanate.

[0066] The raw materials of UV slurry include: 55 parts of photosensitive resin adhesive, 30 parts of ethyl acetate, and 2 parts of light curing agent.

[0067] The reflective film preparation method of this embodiment comprises the following steps: adding the raw materials in the coating liquid into a liquid preparation tank, stirring at 800 rpm for 100 min to form a coating liquid, coating the coating liquid on one side of the reflective base film with a coating thickness of 14 μm, curing at 110° C. for 3 min, and finally aging at 65° C. for 16 h; adding the raw materials of the UV slurry into a liquid preparation tank, stirring at 800 rpm for 100 min to form a UV slurry, coating the UV slurry on the other side of the aged reflective base film with a coating thickness of 2 μm, curing at 80° C. for 3 min, and then passing through a UV curing machine, with the UV energy controlled at 300 mJ / cm 2 , and the speed is 4.5 m / min to obtain a UV adhesive layer, that is, the reflective film of this embodiment. Example 3

[0068] The coating liquid raw materials include: 40 parts of acrylic resin adhesive (hydroxyl value content is 33 mgKOH / g (solid), solid content is 65wt%), 0.3 parts of PU particles (average particle size is 17μm), 24.7 parts of PMMA coated TiO2, 50 parts of ethyl acetate and butyl acetate with a volume ratio of 1:1, 0.7 parts of hexadecyltrimethylammonium chloride antistatic agent, and 4 parts of HDI-based polyisocyanate.

[0069] The raw materials of UV slurry include: 65 parts of photosensitive resin adhesive, 42 parts of ethyl acetate, and 4 parts of light curing agent.

[0070] The reflective film preparation method of this embodiment comprises the following steps: adding the raw materials in the coating liquid into a liquid preparation tank, stirring at 2000 rpm for 30 minutes to form a coating liquid, coating the coating liquid on one side of the reflective base film with a coating thickness of 15 μm, curing at 130° C. for 2 minutes, and finally aging at 55° C. for 24 hours; adding the raw materials of the UV slurry into a liquid preparation tank, stirring at 2000 rpm for 30 minutes to form a UV slurry, coating the UV slurry on the other side of the aged reflective base film with a coating thickness of 4 μm, curing at 90° C. for 1 minute, and then passing through a UV curing machine, with the UV energy controlled at 500 mJ / cm 2 , and the speed is 4.2 m / min to obtain a UV adhesive layer, that is, the reflective film of this embodiment. Example 4

[0071] The only difference between Example 4 and Example 1 is that the hydroxyl value content of the acrylic resin adhesive in Example 4 is 10 mgKOH / g (solid), and the solid content is 65 wt %. The rest is the same as Example 1. Example 5

[0072] The difference between Example 5 and Example 1 is that Example 5 uses PMMA-coated hollow TiO2 particles instead of PMMA-coated TiO2 particles, and the rest is the same as Example 1.

[0073] Comparative Example 1

[0074] The difference between Comparative Example 1 and Example 1 is that 20 parts of PMMA-coated TiO2 are used in the coating raw materials of Comparative Example 1 to replace 0.2 parts of PU particles and 19.8 parts of PMMA-coated TiO2 in Example 1, and the rest is the same as Example 1.

[0075] Comparative Example 2

[0076] In the coating raw material of Comparative Example 2, PMMA particles (average particle size of 17 μm) are used to replace the PU particles (average particle size of 17 μm) of Example 1, and the rest is the same as Example 1.

[0077] Comparative Example 3

[0078] In the coating raw material of Comparative Example 3, TiO2 is used to replace the PMMA-coated TiO2 in Example 1, and the rest is the same as Example 1.

[0079] Comparative Example 4

[0080] In the coating raw material of Comparative Example 4, PBMA-coated TiO2 is used to replace the PMMA-coated TiO2 of Example 1, and the rest is the same as Example 1.

[0081] The difference between the preparation method of PBMA coated TiO2 and PMMA coated TiO2 is that n-butyl methacrylate is used instead of methyl methacrylate in the preparation method of PBMA coated TiO2.

[0082] Comparative Example 5

[0083] In the coating raw material of Comparative Example 5, PU particles (average particle size of 4 μm) are used to replace the PU particles (average particle size of 17 μm) in Example 1, and the rest is the same as Example 1.

[0084] Comparative Example 6

[0085] The difference between Comparative Example 6 and Example 1 is that in the coating raw materials of Comparative Example 6, 1 part of PU particles and 19 parts of PMMA-coated TiO2 are used to replace 0.2 parts of PU particles and 19.8 parts of PMMA-coated TiO2 in Example 1, and the rest is the same as Example 1.

[0086] Comparative Example 7

[0087] The difference between Comparative Example 7 and Example 1 is that Comparative Example 7 does not have a UV adhesive layer.

[0088] Comparative Example 8

[0089] In the coating raw material of Comparative Example 8, hollow TiO2 is used to replace the PMMA-coated hollow TiO2 in Example 5, and the rest is the same as Example 1.

[0090] The performance tests were conducted on the reflective films of Examples 1-5 and Comparative Examples 1-8. The specific test process is as follows and the results are shown in Table 1.

[0091] Scratch resistance test

[0092] Use a scratch tester to test 50 times back and forth at a speed of 14m / min under a pressure of 1000g to observe whether the light guide plate and the coated reflective film are scratched. The light guide plate uses a hot-pressed PMMA light guide plate-HIghbroad.

[0093] Anti-whitening test

[0094] Fix a screw on the jig; assemble the reflective film to be tested on the backlight module and place it on the jig, press two 1KG weights on the backlight module; light up the jig and observe whether there are white spots on the backlight emitting surface corresponding to the screw. Evaluate according to the anti-whitening situation:

[0095] LEV.1: No white spots observed on the light guide plate;

[0096] LEV.2: White spots are faintly visible when viewed from the light guide plate;

[0097] LEV.3: White spots are clearly visible when observed from the light guide plate.

[0098] Table 1 Performance data of reflective films of embodiments and comparative examples

[0099]

[0100] The reflective films prepared in Examples 1-3 have excellent reflectivity, scratch resistance and anti-whitening properties. Example 4 uses an acrylic resin adhesive with a hydroxyl value of 10 mg KOH / g. After a scratch test, there are slight scratches on the light guide plate. Comparison between Example 4 and Example 1 shows that the acrylic resin adhesive with a higher hydroxyl value used in coating the reflective film has a rigid adhesive layer that can effectively restrain the particles inside the adhesive layer, preventing the particles from breaking through the adhesive layer and scratching the light guide plate.

[0101] In Example 5, PMMA is used to coat hollow TiO2 particles. Compared with the PMMA-coated TiO2 particles in Example 1, the reflectivity of the reflective film prepared by the PMMA-coated TiO2 particles is as high as 96.87%. The incident light is scattered multiple times on the outer and inner surfaces of titanium dioxide, thereby obtaining a higher reflectivity.

[0102] Compared with Example 1, PU particles are not added in Comparative Example 1, and the anti-whitening effect of the reflective film is greatly affected, and obvious white spots can be observed on the light guide plate. Comparative Example 2 uses PMMA particles to replace PU particles. PMMA particles are rigid particles. The presence of large-sized PMMA particles in the reflective film is easy to scratch the light guide plate, and the anti-whitening effect of large-sized PMMA is not as good as that of PU particles. The TiO2 in Comparative Example 3 is not coated with PMMA, which is not conducive to the reflection of light, and the reflectivity of the reflective film prepared therefrom is reduced to 95.87%. Comparative Example 4 uses PBMA to coat TiO2, and its reflectivity is lower than that of PMMA-coated TiO2. This is because the refractive index of PMMA and acrylic adhesive is similar, and the incident light will not be greatly refracted. The incident light from air-acrylic adhesive-PMMA-titanium dioxide is more concentrated than air-acrylic adhesive-PBMA-titanium dioxide; in addition, PMMA is a very excellent transparent material, which is conducive to the incident light passing through PMMA and concentrating on TiO2. Comparative Example 5 uses small-sized PU particles, and the anti-whitening effect of the reflective film is greatly reduced. The reflective film of Comparative Example 6 has too much PU particles, and the conductive plate is slightly scratched. The excessive PU particles lead to too little PMMA-coated TiO2 content, and the reflectivity is reduced. Comparative Example 7 does not apply a UV adhesive layer, and the anti-whitening effect is reduced.

[0103] After the non-hollow TiO2 was coated with PMMA (Example 1), the reflectivity increased by 0.5% relative to the uncoated non-hollow TiO2 (Comparative Example 3); after the hollow TiO2 was coated with PMMA (Example 5), the reflectivity increased by 0.8% relative to the uncoated hollow TiO2 (Comparative Example 8); this means that the effect of PMMA-coated hollow TiO2 on improving the reflectivity is significantly better than that of PMMA-coated non-hollow TiO2.

[0104] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0105] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0106] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A high brightness scratch-resistant coated reflective film, It is characterized in that The invention comprises a UV adhesive layer, a reflective base film and a coating layer in sequence, wherein the coating layer comprises an adhesive layer and composite particles, the adhesive layer is bonded to the surface of the reflective base film, and the composite particles are distributed in the adhesive layer; The composite particles include polyurethane particles and polymethyl methacrylate-coated TiO 2 particle; The average particle size of the polyurethane particles is 10-30 μm, and the polymethyl methacrylate coated TiO 2 The average particle size is 1~8μm; Polyurethane particles and polymethyl methacrylate coated TiO 2 The mass ratio of particles is 1:70~120.

2. A high brightness scratch-resistant coated reflective film according to claim 1, It is characterized in that The polymethyl methacrylate coated TiO 2 The method for preparing the particles comprises the following steps: TiO 2 The particles are dispersed in an acid solution for pretreatment; Pretreated TiO 2 The particles are dispersed in an organic solvent, and then acetic acid and azobisisobutyronitrile are added. When the temperature rises to 50-80°C, methyl methacrylate is added to react. After the reaction, the product was washed and centrifuged to obtain polymethyl methacrylate-coated TiO 2 particle.

3. A high brightness scratch-resistant coated reflective film according to claim 2, It is characterized in that The pH of the acid solution is 1 to 3; The volume of the acid solution and the TiO 2 The mass ratio of particles is 5~500ml:1g; Organic solvent: TiO 2 : The mass ratio of acetic acid: methyl methacrylate: azobisisobutyronitrile is 240: (1.5~15): (0.5~5): (5~50): (0.2~3); Add methyl methacrylate and react for 5 to 30 hours.

4. A high brightness scratch-resistant coated reflective film according to claim 1 or 2, It is characterized in that The TiO 2 The particles are hollow TiO 2 Particles, the polymethyl methacrylate coated TiO 2 The particles are hollow TiO coated with polymethyl methacrylate 2 particle.

5. The high brightness scratch-resistant coated reflective film according to claim 1, It is characterized in that The coating layer is prepared from a coating liquid, which includes: 20 to 40 parts of an adhesive, 10 to 30 parts of composite particles, 35 to 55 parts of a solvent, and 1 to 5 parts of a curing agent.

6. A high brightness scratch-resistant coated reflective film according to claim 5, It is characterized in that The adhesive is an acrylic resin adhesive, and the hydroxyl content of the acrylic resin adhesive is 20-40 mg KOH / g solid; The solvent is one or more of ethyl acetate, butyl acetate and butanone; The curing agent is aliphatic polyisocyanate.

7. The high brightness scratch-resistant coated reflective film according to claim 1, It is characterized in that The UV adhesive layer is prepared from UV slurry, and the UV slurry includes: 30-45 parts of solvent, 1-5 parts of light curing agent and 50-70 parts of photosensitive resin adhesive.

8. A high brightness scratch-resistant coated reflective film according to claim 7, It is characterized in that The solvent is one or more of ethyl acetate, butyl acetate and butanone; The photocuring agent is an aliphatic polyisocyanate; The photosensitive resin adhesive is trifunctional polyurethane acrylate with a solid content of 25~65wt%.

9. A method for preparing a high brightness scratch-resistant coating reflective film as claimed in claim 1, It is characterized in that The following steps are involved: Add the raw materials in the coating liquid into the liquid preparation tank, stir for 5 to 300 minutes to form the coating liquid, apply the coating liquid on one side of the reflective base film, obtain the coating layer after curing, and then ripen; The raw materials of UV slurry are added into a liquid preparation tank and stirred for 5 to 300 minutes to form UV slurry. The UV slurry is coated on the other side of the matured reflective base film. After pre-curing and UV curing, a UV adhesive layer is obtained, that is, the high-brightness scratch-resistant coated reflective film is obtained.

10. The preparation method according to claim 9, It is characterized in that The coating liquid is coated on one side of the reflective base film to a thickness of 10 to 15 μm; The curing temperature of the coating liquid is 100~120℃, and the curing time is 1~5min; The aging temperature is 50~70℃ and the aging time is 10~30h; The thickness of the UV slurry coated on the other side of the matured reflective base film is 1~5μm; The pre-curing temperature of UV slurry is 70~90℃, and the pre-curing time is 0.5~4min; UV energy for UV curing is 200~800mJ / cm 2 .

Citation Information

Patent Citations

  • Optical thin film with high covering power and high luminance and display device comprising optical thin film

    CN102759761A

  • High-luminance diffusion silver-plated reflective film and preparation method thereof

    CN106680919A

  • Layered coating type scratch-resistant coating reflecting film and preparation method thereof

    CN114779378A

  • Coated reflective film based on multi-morphology particle coating and preparation method thereof

    CN117555060A

  • Manufacturing method of scratch-resistant resin plate having glare-proof property

    JP2008296428A