Conductive slurry preparation process based on particle size control method
By controlling the particle size preparation process and combining silver powder, palladium powder, tin powder, graphene and other materials, the problem of difficult to balance conductivity, stability and corrosion resistance of conductive slurry is solved, and high-performance conductive slurry is achieved. The preparation of materials is suitable for use in the electronics industry and other fields.
Patent Information
- Application Number
- CN202411072165.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for traditional conductive slurry formulas to take into account conductivity, stability and corrosion resistance, and there are challenges in uniform dispersion of nanomaterials in the slurry, which affects the improvement of conductive performance.
Using a conductive slurry preparation process based on the particle size control method, through the combination of silver powder, palladium powder, tin powder and graphene and other materials, combined with the use of dispersants, adhesives and additives, through steps such as stirring, grinding and filtration , to achieve uniform dispersion and improved stability of materials.
It achieves improved conductivity, enhanced stability and corrosion resistance, extends the service life of the slurry, improves dispersion, viscosity and processability, reduces resistivity, and is suitable for printing and spraying processes.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of conductive pastes, and in particular relates to a conductive paste preparation process based on a particle size control method. Background Art
[0002] In the electronics industry, conductive paste is a key functional material, widely used in integrated circuits, solar cells, capacitors and other fields. Traditional conductive paste formulations often focus on improving a single performance, such as conductivity or stability, but often find it difficult to take into account other properties. In recent years, with the rapid development of nanotechnology, the introduction of new nanomaterials such as graphene has provided new ideas for improving the performance of conductive pastes; however, although the introduction of nanomaterials such as graphene has made it possible to improve the performance of conductive pastes, there are still many challenges in practical applications. First, the uniform dispersion of nanomaterials is the key to preparing high-performance conductive pastes, but how to achieve uniform dispersion of nanomaterials in the paste is still a technical problem. Secondly, how to improve the stability and corrosion resistance of the paste and extend its service life while ensuring the conductive performance is also a problem to be solved. Therefore, developing a conductive paste formulation with excellent comprehensive performance has important practical significance and application value. Summary of the invention
[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a conductive paste preparation process based on the particle size control method, which effectively solves the problems raised by the background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a process for preparing a conductive paste based on a particle size control method, comprising the following steps:
[0005] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0006] Step 2, solvent pretreatment: Before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 200-300 rpm to remove existing bubbles and impurities. Continue stirring for 5-10 minutes until the solvent becomes clear and transparent;
[0007] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 400-500rpm, and continue stirring for 10-15 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0008] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 15-20 minutes to ensure that the dispersant and adhesive are fully mixed;
[0009] Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 20-30 minutes to ensure that the additives are fully mixed and work properly;
[0010] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 1-2 hours; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0011] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0012] Preferably, the materials in step 1 include the following components in parts by weight:
[0013] 50-60 parts of silver powder, 5-6 parts of palladium powder, 3-5 parts of tin powder, 3-7 parts of graphene, 1-3 parts of dispersant, 3-5 parts of adhesive, 1-3 parts of additives, and 30-40 parts of acetone.
[0014] Preferably, the materials in step 1 include the following components in parts by weight:
[0015] 55 parts of silver powder, 5 parts of palladium powder, 4 parts of tin powder, 5 parts of graphene, 2 parts of dispersant, 4 parts of adhesive, 2 parts of additives, and 35 parts of acetone.
[0016] Preferably, the materials in step 1 include the following components in parts by weight:
[0017] 50 parts of silver powder, 5 parts of palladium powder, 3 parts of tin powder, 3 parts of graphene, 1 part of dispersant, 3 parts of adhesive, 1 part of additive, and 30 parts of acetone.
[0018] Preferably, the dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] First, silver powder is used as the main conductive filler to provide excellent conductive properties and ensure the high conductivity of the slurry; the addition of palladium powder and tin powder not only enhances the conductive properties, but also improves the stability and corrosion resistance of the slurry and prolongs its service life; secondly, the addition of graphene can not only enhance the conductivity of the slurry, but also improve the dispersibility and viscosity of the slurry, making the slurry more uniform and stable; in addition, the appropriate addition of dispersants, adhesives and additives further improves the dispersibility, adhesion and processability of the slurry, making the slurry easy to mix, stir and shape during the preparation process. At the same time, these additives can also reduce the resistivity of the slurry and improve the conductive efficiency. Acetone is used as an organic solvent to provide the slurry with good fluidity and wettability, so that the slurry can be evenly covered on the substrate during printing, spraying and other processes to form a continuous and dense conductive layer. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] The present invention relates to a process for preparing a conductive paste based on a particle size control method, comprising the following steps:
[0023] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0024] Step 2, solvent pretreatment: Before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 200-300 rpm to remove existing bubbles and impurities. Continue stirring for 5-10 minutes until the solvent becomes clear and transparent;
[0025] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 400-500rpm, and continue stirring for 10-15 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0026] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 15-20 minutes to ensure that the dispersant and adhesive are fully mixed;
[0027] Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 20-30 minutes to ensure that the additives are fully mixed and work properly;
[0028] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 1-2 hours; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0029] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0030] The materials in step 1 include the following components by weight:
[0031] 50-60 parts of silver powder, 5-6 parts of palladium powder, 3-5 parts of tin powder, 3-7 parts of graphene, 1-3 parts of dispersant, 3-5 parts of adhesive, 1-3 parts of additives, and 30-40 parts of acetone.
[0032] The materials in step 1 include the following components by weight:
[0033] 55 parts of silver powder, 5 parts of palladium powder, 4 parts of tin powder, 5 parts of graphene, 2 parts of dispersant, 4 parts of adhesive, 2 parts of additives, and 35 parts of acetone.
[0034] The materials in step 1 include the following components by weight:
[0035] 50 parts of silver powder, 5 parts of palladium powder, 3 parts of tin powder, 3 parts of graphene, 1 part of dispersant, 3 parts of adhesive, 1 part of additive, and 30 parts of acetone.
[0036] The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0037] Embodiment 1:
[0038] This embodiment relates to a conductive paste preparation process based on a particle size control method, comprising the following steps:
[0039] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0040] Step 2, solvent pretreatment: before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 200 rpm to remove bubbles and impurities. Continue stirring for 10 minutes until the solvent becomes clear and transparent;
[0041] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 400 rpm, and continue stirring for 15 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0042] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 15 minutes to ensure that the dispersant and adhesive are fully mixed;
[0043] Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 20 minutes to ensure that the additives are fully mixed and work properly;
[0044] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 1 hour; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0045] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0046] The materials in step 1 include the following components by weight:
[0047] 50 parts of silver powder, 5 parts of palladium powder, 3 parts of tin powder, 3 parts of graphene, 1 part of dispersant, 3 parts of adhesive, 1 part of additive, and 30 parts of acetone.
[0048] The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0049] Embodiment 2:
[0050] This embodiment relates to a conductive paste preparation process based on a particle size control method, comprising the following steps:
[0051] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0052] Step 2, solvent pretreatment: before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 300 rpm to remove bubbles and impurities. Continue stirring for 5 minutes until the solvent becomes clear and transparent.
[0053] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 500 rpm, and continue stirring for 10 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0054] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 20 minutes to ensure that the dispersant and adhesive are fully mixed;
[0055] Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 30 minutes to ensure that the additives are fully mixed and work properly;
[0056] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 2 hours; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0057] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0058] The materials in step 1 include the following components by weight:
[0059] 60 parts of silver powder, 6 parts of palladium powder, 5 parts of tin powder, 7 parts of graphene, 3 parts of dispersant, 5 parts of adhesive, 3 parts of additives, and 40 parts of acetone.
[0060] The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0061] Embodiment 3:
[0062] This embodiment relates to a conductive paste preparation process based on a particle size control method, comprising the following steps:
[0063] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0064] Step 2, solvent pretreatment: before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 250 rpm to remove existing bubbles and impurities. Continue stirring for 8 minutes until the solvent becomes clear and transparent;
[0065] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 450 rpm, and continue stirring for 13 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0066] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 16 minutes to ensure that the dispersant and adhesive are fully mixed;
[0067] Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 25 minutes to ensure that the additives are fully mixed and work properly;
[0068] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 1.5 hours; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0069] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0070] The materials in step 1 include the following components by weight:
[0071] 55 parts of silver powder, 5 parts of palladium powder, 4 parts of tin powder, 5 parts of graphene, 2 parts of dispersant, 4 parts of adhesive, 2 parts of additives, and 35 parts of acetone.
[0072] The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0073] Embodiment 4:
[0074] This embodiment relates to a conductive paste preparation process based on a particle size control method, comprising the following steps:
[0075] Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities;
[0076] Step 2, solvent pretreatment: before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 200 rpm to remove bubbles and impurities. Continue stirring for 10 minutes until the solvent becomes clear and transparent;
[0077] Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 480 rpm, and continue stirring for 15 minutes to ensure that the solid materials are initially dispersed in the solvent;
[0078] Step 4: Adding dispersant and adhesive: Add dispersant and adhesive to the slurry according to the formula ratio; continue stirring for 19 minutes to ensure that the dispersant and adhesive are fully mixed;
[0079] Step 5, adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 22 minutes to ensure that the additives are fully mixed and work;
[0080] Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 2 hours; after grinding, filter the slurry with a filter to remove large particles and impurities;
[0081] Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
[0082] The materials in step 1 include the following components by weight:
[0083] 57 parts of silver powder, 5 parts of palladium powder, 3 parts of tin powder, 4 parts of graphene, 3 parts of dispersant, 4 parts of adhesive, 1 part of auxiliary agent, and 33 parts of acetone.
[0084] The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
[0085] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A conductive paste preparation process based on particle size control method, It is characterized in that The following steps are involved: Step 1, material preparation: prepare all required materials, including silver powder, palladium powder, tin powder, graphene, dispersant, adhesive, additive and acetone; ensure that the quality of all materials meets the standards and is free of impurities; Step 2, solvent pretreatment: Before starting mixing, pour the acetone solvent into a clean stirring container and use a stirrer to stir at a low speed of 200-300 rpm to remove existing bubbles and impurities. Continue stirring for 5-10 minutes until the solvent becomes clear and transparent; Step 3: Mixing solid materials: weigh silver powder, palladium powder, tin powder and graphene according to the formula ratio, and slowly add them into the stirring acetone solvent, increase the stirring speed to 400-500rpm, and continue stirring for 10-15 minutes to ensure that the solid materials are initially dispersed in the solvent; Step 4: Adding dispersant and adhesive: adding dispersant and adhesive into the slurry according to the formula ratio; Continue stirring for 15-20 minutes to ensure that the dispersant and binder are fully mixed; Step 5: Adding additives: Add the additives to the slurry according to the formula ratio and continue stirring for 20-30 minutes to ensure that the additives are fully mixed and work properly; Step 6, grinding and filtering: pour the mixed slurry into a grinder and grind it for 1-2 hours; After grinding, the slurry is filtered using a screen or filter to remove large particles and impurities; Step 7, Storage and Testing: Pour the filtered slurry into a clean storage container and seal it for storage.
2. A process for preparing a conductive paste based on a particle size control method according to claim 1, It is characterized in that The materials in step 1 include the following components by weight: 50-60 parts of silver powder, 5-6 parts of palladium powder, 3-5 parts of tin powder, 3-7 parts of graphene, 1-3 parts of dispersant, 3-5 parts of adhesive, 1-3 parts of additives, and 30-40 parts of acetone.
3. A process for preparing a conductive paste based on a particle size control method according to claim 2, It is characterized in that The materials in step 1 include the following components by weight: 55 parts of silver powder, 5 parts of palladium powder, 4 parts of tin powder, 5 parts of graphene, 2 parts of dispersant, 4 parts of adhesive, 2 parts of additives, and 35 parts of acetone.
4. A process for preparing a conductive paste based on a particle size control method according to claim 2, It is characterized in that The materials in step 1 include the following components by weight: 50 parts of silver powder, 5 parts of palladium powder, 3 parts of tin powder, 3 parts of graphene, 1 part of dispersant, 3 parts of adhesive, 1 part of additive, and 30 parts of acetone.
5. The process for preparing a conductive paste based on a particle size control method according to claim 1, It is characterized in that The dispersant is polyoxyethylene alcohol, the adhesive is polypropylene, and the auxiliary agent is sodium silicate.
Citation Information
Patent Citations
High-conductivity and low-temperature cured conductive paste and preparation method thereof
CN108133768A
Lithium ion battery, negative electrode, negative electrode conductive paste and preparation method of negative electrode conductive paste
CN108598404A
Welding paste
CN109822259A
Conductive paste for in-mold electronic technology (IME) and preparation method of conductive paste
CN111681804A
Quick-drying silver paste for graphene heating film and preparation method of quick-drying silver paste
CN113077924A