Manufacturing method of Halbach array magnet assembly

Through the manufacturing method of Halbeck array magnet components, the problem of difficulty in controlling the thickness and bonding effect of single magnets in the traditional method is solved, the dimensional accuracy and bonding uniformity of the components are achieved, the deformation problem is reduced, and the quality of the product is improved. and service life.

CN118737679AActive Publication Date: 2024-10-01HANGZHOU MAGMAX TECH CO LTD

Patent Information

Application Number
CN202410932842.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

For traditional Halbeck array magnet components, it is difficult to accurately control the thickness of the single magnet and the bonding effect between magnets in small products, resulting in uneven size and glue shedding problems. In addition, serious deformation occurs during high-temperature welding, resulting in product failure.

Method used

The manufacturing method of Halbach array magnet components is adopted, including preliminary processing of permanent magnet blanks, marking the bonding surface and non-laminated surface, vacuum pressure diffusion connection, surface processing and integrated magnetization, and controlling the thickness of the adhesive layer and anti-oxidation layer. and materials to ensure component dimensional accuracy and bonding uniformity.

Benefits of technology

The dimensional accuracy control of the Halbeck array magnet assembly is achieved, the bonding uniformity and anti-oxidation effect are enhanced, the deformation problem is reduced, and the service life and processing efficiency of the assembly are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_10
    Figure FT_10
  • Figure FT_11
    Figure FT_11
Patent Text Reader

Abstract

The invention relates to the technical field of Halbach array magnets, and particularly discloses a manufacturing method of a Halbach array magnet assembly, which comprises the following steps of: 1) preliminarily processing a blank material to obtain a permanent magnet blank with the thickness of not more than 1.5 mm and the length-diameter ratio of more than 20; 2) performing Halbach array arrangement, and marking a binding surface and a non-binding surface on the permanent magnet blank; 3) coating a bonding layer on the binding surface, coating an anti-oxidation layer on the non-binding surface, carrying out binding on the binding surface, and carrying out diffusion bonding treatment under vacuum pressurization to obtain an assembly product after heat treatment; 4) processing again to meet the size requirement of the target Halbach array, and forming a semi-finished product of the Halbach array magnet assembly; according to the manufacturing method of the Halbach array magnet assembly, single magnets with the thickness not larger than 1.5 mm and the length-diameter ratio larger than 20 can be evenly and compactly attached in the process of manufacturing the Halbach array magnet assembly, and deformation is not prone to occurring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of Halbach array magnets, and more specifically, to a method for manufacturing a Halbach array magnet assembly. Background Art

[0002] Halbach Array is a magnet structure, which is a nearly ideal structure in engineering. Permanent magnets with different magnetization directions are arranged in a certain order, so that the magnetic field on the working surface is significantly enhanced, while the magnetic field on the non-working surface is significantly weakened. The goal is to use the least amount of magnets to generate the strongest magnetic field, while reducing the impact of the stray field on other components.

[0003] The traditional Halbach array magnet assembly is a magnet assembly that is first processed into a single magnet to a specified size and specification, and then glued and assembled. However, when the required size is smaller, the subsequent assembly process, such as machining and electroplating, can easily cause a large deviation in the already small size, and eventually even easily lead to the formation of a Halbach array magnet assembly that is unqualified.

[0004] In the application field of smaller products such as consumer electronics or small motors, the thickness of the single-piece magnets in the Halbach array magnet assembly and the bonding effect between the magnets are more stringent. If the traditional Halbach array magnet assembly method is used, the possible problems include the following aspects: 1. The processing process has high requirements on the processing size of the single-piece magnet. The thickness of this single-piece magnet is small, so it is difficult to accurately control the thickness uniformity of the glue bonding layer, which easily leads to size differences in the magnet assembly; and after the assembly is assembled, it is difficult to perform fine processing again due to the presence of glue. Therefore, the Halbach array magnet assembly made by this method is very likely to have problems with uneven product size.

[0005] And because each single magnet has a specific magnetization direction, when the arrangement directions of the single magnets are different, there will be a large repulsive force between the magnets, causing the glue to easily fall off, making the Halbach array magnet assembly easily misaligned during operation, thereby damaging the equipment.

[0006] 2. In addition, if the processing of Halbach array magnet components involves processes such as grain boundary diffusion-welding that require high temperature treatment, the temperature conditions usually reach 700-1000℃. The single-piece magnet is too thin and is prone to deformation during high temperature treatment (see Figure 1 and Figure 2 ) eventually leads to welding failure.

[0007] Therefore, the Halbach array magnet assembly obtained by glue assembly is prone to problems such as uneven overall size and glue falling off. When high-temperature treatment processes such as grain boundary diffusion-welding are used, deformation problems are prone to occur, which ultimately leads to unqualified products. Summary of the invention

[0008] In order to reduce the problems of uneven size and glue falling off caused by glue bonding during the process of manufacturing Halbach array magnets using a single-piece magnet (or permanent magnet blank) with a single-piece thickness of no more than 1.5 mm and an aspect ratio of more than 20, and to reduce the problem of magnet deformation caused by grain boundary diffusion-welding operation requirements, the present application provides a method for manufacturing a Halbach array magnet assembly.

[0009] In the first aspect, the present application provides the following technical solutions: The manufacturing method of the Halbach array magnet assembly comprises the following steps: 1) Preliminary processing of the blank material according to size requirements to obtain a permanent magnet blank; 2) Perform Halbach array arrangement and mark the bonding surface and non-bonding surface on the permanent magnet blank; 3) Coating an adhesive layer on the bonding surface of the permanent magnet blank, coating an anti-oxidation layer on the non-bonding surface of the magnet blank, bonding the bonding surfaces, and then performing diffusion bonding treatment under vacuum and pressure conditions to obtain a heat-treated component product; 4) Reprocess the heat-treated component products to meet the size requirements of the target Halbach array, forming a semi-finished Halbach array magnet component; 5) Surface processing of the semi-finished products of Halbach array magnet components; 6) Magnetizing the surface-processed semi-finished Halbach array magnet assembly according to the orientation direction to obtain the Halbach array magnet assembly; The thickness of the permanent magnet blank preliminarily processed in step 1) is not greater than 1.5 mm, and the aspect ratio is greater than 20.

[0010] By adopting the above technical solution, this application mainly manufactures Halbach array magnet components for permanent magnet blanks with a thickness of no more than 1.5 mm and an aspect ratio of more than 20. The main reason is that when the thickness of the permanent magnet blank used as the Halbach array magnet component is no more than 1.5 mm and the aspect ratio is greater than 20, the processing accuracy of the permanent magnet blank is difficult to control, and debonding is prone to occur after integrated magnetization.

[0011] In step 1), the permanent magnet blanks are arranged in a Halbach array according to actual needs, which can be arranged in countless situations. Therefore, in step 2), the bonding surface and non-bonding surface in the arrangement process are marked to facilitate subsequent operations.

[0012] In the process of manufacturing the Halbach array magnet assembly, through the mutual coordination of the materials coated between the bonding surface and the non-bonding surface in step 3), combined with the control of the process conditions during the operation process, the adhesive layer on the bonding surface and the anti-oxidation layer on the non-bonding surface are both denser and less prone to defects, and the coating thickness is also more uniform, which is beneficial to improving the bonding effect and anti-oxidation effect.

[0013] In step 4), the product is processed according to the size requirements of the target product (see Figure 3 ). The uneven anti-oxidation layer on the non-fitting surface is processed flat. Generally, the non-fitting surface has a processing size margin. The thickness direction is processed in place first, so that part of the uneven anti-oxidation layer on the non-fitting surface is removed at the same time. In this application, the permanent magnet blank is first rough-machined and then fine-machined, which is different from the traditional Halbach array magnet manufacturing method.

[0014] In step 5), the surface processing is to chamfer, electroplate or spray the semi-finished product of the Halbach array magnet assembly obtained in step 4) to improve the corrosion resistance and anti-collision ability of the Halbach array magnet assembly, and further improve the service life of the Halbach array magnet assembly.

[0015] Finally, the semi-finished Halbach array magnet assembly obtained after assembly is magnetized as a whole. This operation is more convenient and helps to improve processing efficiency.

[0016] Through the processing of all the above steps, not only can the Halbach array magnet assembly be quickly assembled and dimensional accuracy control be achieved, but the overall bonding uniformity and bonding effect of the Halbach array magnet assembly can also be increased to ensure that the magnet assembly will not be separated from each other due to the repulsive force caused by different orientations between the magnets during subsequent use, resulting in failure.

[0017] Furthermore, the thickness of the permanent magnet blank preliminarily processed in step 1) is 0.15-1.5 mm.

[0018] Since the factory processing mostly uses the above thickness range, the processing method and subsequent assembly of permanent magnet blanks within this thickness range are more familiar. Other sizes can also be processed according to actual requirements.

[0019] Furthermore, in the step three, the thickness of the adhesive layer on the bonding surfaces between adjacent permanent magnet blanks is 0.3 μm-150 μm; and the coating thickness on the non-bonding surfaces is 0.3 μm-200 μm.

[0020] By adopting the above technical solution, when coating on the bonding surface and the non-bonding surface, it is necessary to control the coating thickness of the bonding layer and the anti-oxidation layer, especially the thickness of the bonding layer on the bonding surface, and the thickness of the bonding layer on the bonding surface between adjacent permanent magnet blanks needs to be kept at 0.3-150μm. If the thickness of the bonding layer is too small, different thin magnets cannot be well bonded together, resulting in low bonding strength; if the thickness of the bonding layer is too large, it will first lead to an increase in the cost of the coating material, and secondly, it will cause fluctuations in the size of the magnet assembly.

[0021] Furthermore, the coating thicknesses of the adhesive layer and the anti-oxidation layer in the Halbach array magnet assembly can be kept the same or different.

[0022] Furthermore, in the step three, the thickness of the adhesive layer on the bonding surfaces between adjacent permanent magnet blanks is 2.5 μm-25 μm; and the coating thickness on the non-bonding surfaces is 14.5 μm-60 μm.

[0023] The thickness of the adhesive layer and the anti-oxidation layer commonly used by the applicant are respectively within the above ranges, which is conducive to making the magnet assembly have a better adhesive effect, anti-oxidation effect and maintaining good integrity of the magnet assembly.

[0024] Furthermore, the vacuum degree in step 3) is <1.0E-04, and the pressure is 2-30Mpa.

[0025] By adopting the above technical solution, the vacuum degree and pressure in step 3) are maintained in this state, which is conducive to making the adhesive layer and anti-oxidation layer obtained after coating have good density and uniformity, and are not prone to defects. It is used to reduce the deformation of the thin magnets in the preparation of the Halbach array magnet assembly caused by the high temperature in the subsequent diffusion bonding process, and can optimize the effect of diffusion bonding, and can more lastingly exert the effectiveness of the Halbach array magnet assembly itself.

[0026] Furthermore, in the step 3), the main component of the anti-oxidation layer coated on the non-bonding surface of the permanent magnet blank is metal powder and / or alloy powder, and / or the anti-oxidation layer is a high temperature resistant film layer; The main component of the adhesive layer coated on the bonding surface of the permanent magnet blank is metal powder and / or alloy powder.

[0027] In the present application, a bonding layer is obtained by coating a coating liquid containing metal powder, alloy powder, or both metal powder and alloy powder on the bonding surface, so that the single-piece permanent magnet blank is pasted as required to form a Halbach array magnet assembly.

[0028] The anti-oxidation layer can be obtained by coating a coating liquid containing metal powder, alloy powder, or both metal powder and alloy powder on the non-bonding surface, and can also be obtained by affixing a high-temperature resistant film layer on the non-bonding surface. However, in most cases, coating is preferred.

[0029] Further, the metal element in the metal powder includes one of Tb, Dy, Gd, Ce, Pr, Nd, Al, Cu, Ag, Ni, Zn, Ga, Nb, Co, Sn, and low melting point rare earth alloy powder; the alloy powder is formed by at least two elements of Tb, Dy, Gd, Ce, Pr, Nd, Al, Cu, Ag, Ni, Zn, Ga, Nb, Co, Sn, and low melting point rare earth alloy; The composition of the low melting point rare earth alloy powder is RE-X, wherein RE is at least one of Tb, Dy, Pr, Nd, Gd, and Ce; X is at least one of Fe, Cu, Al, Ni, Sn, Nb, Ga, Ag, and Co; The high temperature resistant film layer includes a high temperature resistant metal film layer and a high temperature resistant ceramic film layer. The high temperature resistant metal film layer is deposited by a high melting point metal. The high melting point metal includes at least one of Ti, Cr, Ta, W, Mo, and V. The high temperature resistant ceramic film layer is a nitride or carbide ceramic film.

[0030] In the present application, when the bonding surface and the non-bonding surface are coated to obtain the bonding layer or the anti-oxidation layer, there are many options for metal powder and alloy powder, and the materials selected for coating on the non-bonding surface and the bonding surface may be the same or different.

[0031] It is also feasible to form a high temperature resistant film layer as an anti-oxidation layer by deposition on the non-bonding surface.

[0032] On the non-bonded surface, whether the anti-oxidation layer is formed by coating or deposition, the non-bonded surface can have a better anti-oxidation effect and can also reduce the deformation of the magnet during the high-temperature diffusion bonding process.

[0033] Furthermore, the particle size of the metal powder or alloy powder used for coating on the non-bonding surface is 2-50 μm; the particle size of the metal powder or alloy powder used for coating on the bonding surface is 2-10 μm.

[0034] By adopting the above technical solution, the adhesive layer and anti-oxidation layer coated on the non-bonding surface and the bonding surface can be made more uniform, thereby increasing the bonding effect and density between the single-piece magnets, and maintaining good anti-oxidation effect on the non-bonding surface, thereby reducing the deformation of the magnet during the high-temperature diffusion bonding process.

[0035] Furthermore, the coating liquid used when coating the adhesive layer is composed of metal powder and / or alloy powder and a solvent, and the solvent is at least one of anti-oxidation glue and ethanol; The coating liquid used when coating the anti-oxidation layer consists of metal powder and / or alloy powder and pinene alcohol.

[0036] By adopting the above technical scheme, the metal powder and / or alloy powder is fully dispersed through the solvent. When selecting the solvent, it can be adjusted according to the selected metal powder and / or alloy powder, so that the final coating liquid has a uniform texture and is easier to coat, thereby making the texture of the final bonding layer and anti-oxidation layer more uniform, improving the anti-oxidation effect of the magnet during the high-temperature diffusion bonding process, and further reducing the deformation of the magnet during the high-temperature diffusion bonding process.

[0037] In summary, this application has the following beneficial effects: In the present application, the non-bonding surface and the bonding surface are respectively coated, the heat treatment is limited by vacuum and pressure, and the Halbach array magnet assembly is subjected to diffusion bonding treatment, so that the single-piece magnet with a single-piece thickness of no more than 1.5 mm and an aspect ratio of more than 20 can not only be evenly and densely bonded during the manufacturing process of the Halbach array magnet assembly, but also not easily deformed.

[0038] Furthermore, the present application limits the materials used for coating, thereby achieving a good bonding effect of the magnets in the obtained Halbach array magnet assembly. At the same time, since the Halbach array magnet assembly is more regular after heat treatment, subsequent reprocessing is more convenient, reducing material waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 , Side view of the Halbach array magnet assembly prepared by grain boundary diffusion process before and after deformation.

[0040] Figure 2 , front view of the Halbach array magnet assembly prepared by grain boundary diffusion process before and after deformation.

[0041] Figure 3 , a schematic diagram of the process of dimensional processing as required in this application.

[0042] Figure 4 , the arrangement diagram and orientation direction of the Halbach array magnet assembly in Example 1.

[0043] Figure 5 , the arrangement diagram and orientation direction of the Halbach array magnet assembly in Example 3.

[0044] Figure 6 , the arrangement diagram and orientation direction of the Halbach array magnet assembly in Example 4.

[0045] Figure 7 , the arrangement diagram and orientation direction of the Halbach array magnet assembly in Example 5.

[0046] Figure 8 , surface morphology of the test sample in Example 4.

[0047] Fig. 9 , fracture morphology of the test sample in Example 4 ×50.

[0048] Fig.10 , fracture morphology of the test sample in Example 4 × 100.

[0049] Fig.11 , fracture morphology of the test sample in Example 4 × 500.

[0050] Fig.12 , morphology of the test sample after fracture grinding in Example 5 ×500.

[0051] Fig.13 , morphology of the test sample after fracture grinding in Example 6 ×500. DETAILED DESCRIPTION Example

[0052] Embodiment 1: A method for manufacturing a Halbach array magnet assembly, comprising the following steps: 1) Process the magnet blank according to size requirements.

[0053] 2) Arrange the three single-piece permanent magnet blanks in a Halbach array (arrange according to the Halbach array structure), as shown in the following diagram: Figure 1 As shown, the thickness of each single permanent magnet blank is 1.5 mm, the aspect ratio is 34.0, and the size specifications of the single permanent magnet blank from left to right are: 51*1.5*36.5M, 51*1.5M *36.5, 51*1.5*36.5M, and the arrow direction represents the orientation direction. In addition, the bonding surface (i.e., the surface bonded to the adjacent magnet blank) and the non-bonding surface (the surface other than the bonding surface) are marked on each magnet blank.

[0054] 3) An adhesive layer is coated on the bonding surface of the magnet blank, and an anti-oxidation layer is coated on the non-bonding surface of the magnet blank, and then the product is diffusion-bonded under vacuum / high pressure conditions (pressure is 2.03 MPa, vacuum is 9.5×10E-5).

[0055] Among them, the non-bonding surface is provided with an anti-oxidation layer with a thickness of 20±2.0 μm by magnetron sputtering, and the material of the anti-oxidation layer is Al powder; The material used for the adhesive layer coated on the bonding surface is TbFe alloy powder. The adhesive layer coating liquid is first mixed in the ratio of TbFe alloy powder (g): ethanol (ml) = 1:2, and then manually coated. The thickness of the coated adhesive layer is 15±5.0μm.

[0056] The parameters used in the above magnetron sputtering are: argon pressure 0.02 Torr, voltage 1000 V, and current 0.1 A.

[0057] And the specific operation of diffusion connection is: The stacked magnets were fixed and placed in a diffusion furnace. Argon was first introduced into the diffusion furnace until the pressure inside the furnace reached 2.0 MPa. The temperature was raised to 650°C for heat treatment for 30 minutes. The temperature was then raised to 900°C for heat treatment for 20 hours, ensuring that the vacuum was <1.0E-04. The magnets were finally transferred to a tempering furnace and tempered at 480°C for 4 hours.

[0058] 4) Process the product after the above heat treatment to the size of the target array. This processing is only surface micro-machining, and the slightly uneven areas will be processed without affecting the role of the anti-oxidation layer and the adhesive layer, forming a Halbach array magnet semi-finished product.

[0059] 5) Surface processing of the Halbach array magnet semi-finished products.

[0060] 6) Magnetizing the surface-processed Halbach array magnet semi-finished product in one piece to obtain a Halbach array magnet assembly.

[0061] Example 2: A method for manufacturing a Halbach array magnet assembly. The Halbach array arrangement is the same as that in Example 1. The main differences from Example 1 are: the thickness of each single permanent magnet blank is 0.7 mm, the aspect ratio is 21.4, and the size specifications of the single permanent magnet blanks from left to right are: 15*5.87M*0.7, 15*5.87*0.7M, 15*5.87M*0.7.

[0062] In step 3), the anti-oxidation layers coated on the non-bonding surface by magnetron sputtering are respectively a Dy layer and an Al layer from the inside to the outside, and the thickness of the Al layer is 10±1.0 μm, and the thickness of the Dy layer is 3±0.5 μm.

[0063] The adhesive layer coated on the bonding surface by magnetron sputtering is a Dy layer, and the thickness of the Dy layer is 3±0.5 μm.

[0064] Embodiment 3: A method for manufacturing a Halbach array magnet assembly, which differs from Embodiment 1 in that: three single-piece permanent magnet blanks are arranged in a Halbach array, as shown in the following diagram: Figure 2 The thickness of each single permanent magnet blank is 0.5 mm, the aspect ratio is 104.0, and the size specifications of the single permanent magnet blank from left to right are: 52*39.9*0.5M; 52*39.9M*0.5; 52*39.9*0.5M.

[0065] In step 3), an anti-oxidation layer with a thickness of 15±2.0 μm is obtained on the non-bonding surface by magnetron sputtering, wherein the raw material is Al powder.

[0066] The bonding surface is provided with a bonding layer with a thickness of 3±0.5 μm by magnetron sputtering, wherein the raw material is Al powder.

[0067] Embodiment 4: A method for manufacturing a Halbach array magnet assembly, which differs from Embodiment 1 in that: 5 single-piece permanent magnet blanks are arranged in a Halbach array, as shown in the following diagram: Figure 3 The thickness of each single permanent magnet blank is 0.43 mm, the aspect ratio is 117.7, and the size specifications of the single permanent magnet blank from left to right are: 50.6*0.43*43.2M; 50.6*0.43M*43.2; 50.6*0.43*43.2M; 50.6*0.43M*43.2; 50.6*0.43*43.2M.

[0068] In step 3), the non-bonding surface is manually coated to obtain an anti-oxidation layer. The specific operation is: first, PrNd alloy powder (g): pine oil (g) = 5:1 is fully mixed to obtain an anti-oxidation layer coating liquid, and then manually coated to obtain an oxide layer (PrNd layer) with a thickness of 15±2.0μm.

[0069] PrTbAl alloy powder and Cu powder were mixed in a mass ratio of 2:1 to form a mixed metal powder; then the mixed metal powder (g): anti-oxidation glue (g): alcohol (ml) = 50:1:200 were fully mixed to obtain an adhesive layer coating liquid. The adhesive layer was applied to the bonding surface by manual coating and bonding was performed to finally obtain an adhesive layer with a thickness of 3±0.5μm.

[0070] During the diffusion bonding process of step 5), the stacked magnets are fixed and placed in a diffusion furnace. Argon gas is first introduced into the diffusion furnace until the pressure in the furnace reaches 2.0 MPa, and the temperature is raised to 650°C for heat treatment for 30 minutes; then the temperature is raised to 810°C for heat treatment for 20 hours, ensuring that the vacuum is <1.0E-04; finally, the magnets are transferred to a tempering furnace and tempered at 480°C for 4 hours.

[0071] Embodiment 5: A method for manufacturing a Halbach array magnet assembly, which differs from Embodiment 1 in that: 4s pieces of monolithic permanent magnet blanks are arranged in a Halbach array, as shown in the following diagram: Figure 4 The thickness of each single permanent magnet blank is 0.2 mm, the aspect ratio is 253.0, and the size specifications of the single permanent magnet blank from left to right are: 50.6*0.20*43.2M; 50.6*0.20M*43.2; 50.6*0.20M*43.2; 50.6*0.20*43.2M.

[0072] In step 3), the non-bonding surface is manually coated to obtain an anti-oxidation layer. The specific operation is: first, PrNd alloy powder (g): pine oil (g) = 5:1 is fully mixed to obtain an anti-oxidation layer coating liquid, and then manually coated to obtain an oxide layer (PrNd layer) with a thickness of 50±10.0μm.

[0073] Under nitrogen protection, DyHx alloy powder (g): ethanol (ml) = 1:2 was mixed to form an adhesive layer coating liquid, which was manually coated on the bonding surface and bonded to finally obtain an adhesive layer with a thickness of 15±5.0 μm.

[0074] During the diffusion bonding process of step 5), the stacked magnets are fixed and placed in a diffusion furnace. Argon gas is first introduced into the diffusion furnace until the pressure in the furnace reaches 2.0 MPa, and the temperature is raised to 650°C for heat treatment for 30 minutes; then the temperature is raised to 810°C for heat treatment for 20 hours, ensuring that the vacuum is <1.0E-04; finally, the magnets are transferred to a tempering furnace and tempered at 480°C for 4 hours.

[0075] Example 6: A method for manufacturing a Halbach array magnet assembly, which differs from Example 3 in that the thickness of each single permanent magnet blank (from left to right) is 0.15 mm (corresponding to a length-to-diameter ratio of 337.3), 0.15 mm (corresponding to a length-to-diameter ratio of 337.3), and 0.4 mm (corresponding to a length-to-diameter ratio of 126.5), and the size specifications of the single permanent magnet blank are, from left to right, 50.6*0.15M*43.2; 50.6*0.15*43.2M; 50.6*0.40M*43.2.

[0076] In step 3), the non-bonding surface is manually coated to obtain an anti-oxidation layer. The specific operation is: first, PrNd alloy powder (g): pine oil (g) = 5:1 is fully mixed to obtain an anti-oxidation layer coating liquid, and then manually coated to obtain an oxide layer (PrNd layer) with a thickness of 50±10.0μm.

[0077] The TbFe alloy powder and the Ag powder are mixed at a mass ratio of 2:1 to obtain a mixed metal powder; Then, the mixed metal powder (g): anti-oxidation glue (g): ethanol (ml) = 50:1.0:200 is fully mixed to form an adhesive layer coating liquid, which is manually coated on the bonding surface and bonded to finally obtain an adhesive layer with a thickness of 20±5.0 μm.

[0078] During the diffusion bonding process of step 5), the stacked magnets are fixed and placed in a diffusion furnace. Argon is first introduced into the diffusion furnace until the pressure in the furnace reaches 2.0 MPa, and the temperature is raised to 650°C for heat treatment for 30 minutes; then the temperature is raised to 810°C for heat treatment for 20 hours, ensuring that the vacuum is <1.0E-04; finally, the magnets are transferred to a tempering furnace and tempered at 480°C for 4 hours.

[0079] The diffusion bonding processes used in the above-mentioned embodiments 1-6 are all feasible and the diffusion bonding is successful.

[0080] The heat-treated components after the diffusion bonding process in Examples 4-6 were used as test samples, and the results obtained by observation under a microscope were as follows: Figure 6-Figure 13 shown.

[0081] Figure 8 This is a surface morphology diagram of the test sample in Example 4; Fig. 9 This is a fracture morphology diagram of the test sample in Example 4 after being cut by a tool according to size requirements; Figure 10-11 for Fig. 9 Magnified image of .

[0082] from Figure 8 It can be seen that the thickness of each layer of the bonding surface coating is relatively uniform. Fig. 9 It can be seen that the connection between the single permanent magnet blanks is good, uniform and dense, and the semi-finished Halbach array magnet assembly has good integrity. Figure 10-11 It can be more clearly seen that the bonding between the single-piece permanent magnet blanks is uniform and the bonding effect is good.

[0083] Fig.12 This is an enlarged view of the fracture morphology of the test sample in Example 5 after being cut by a tool according to size requirements.

[0084] from Fig.12It can be seen that the adjacent single-piece permanent magnet blanks are closely fitted together, so that the composed magnet assembly has better integrity, and such a magnet assembly is less likely to deform.

[0085] Fig.13 This is an enlarged view of the fracture morphology of the test sample in Example 6 after being cut by a tool according to size requirements.

[0086] from Fig.13 It can be seen that the adjacent single-piece permanent magnet blanks are closely fitted together, so that the composed magnet assembly has better integrity, and such a magnet assembly is less likely to deform.

[0087] Comparative Example 1: The manufacturing method of the Halbach array magnet assembly is different from that of Example 2 in that: In step 3), no anti-oxidation layer is coated on the non-bonding surface; the adhesive layer coated on the bonding surface by magnetron sputtering is a Dy layer, and the thickness of the Dy layer is 3±0.5 μm.

[0088] Comparative Example 2: The manufacturing method of the Halbach array magnet assembly is different from that of Example 1 in that the magnets with different magnetization directions are first magnetized, and then the monolithic permanent magnets are bonded with anti-oxidation glue to form a magnetic assembly with a specific magnetic field distribution, and the thickness of the anti-oxidation glue layer is 15±5.0μm.

[0089] Comparative Example 3: The manufacturing method of the Halbach array magnet assembly is different from that of Example 1 in that the coating thickness of the non-bonding surface and the bonding surface is 0.2 μm.

[0090] Comparative Example 4: A method for manufacturing a Halbach array magnet assembly, which differs from Example 1 in that the coating thickness of the non-bonding surface and the bonding surface is 201 μm.

[0091] The samples before diffusion bonding treatment in Examples 1-6 and Comparative Examples 1-4 were subjected to overall magnet flatness test and the data were recorded; the test samples 1-6 and control samples 1-4 finally obtained in Examples 1-6 and Comparative Examples 1-4 were again subjected to magnet flatness test and the data were recorded, see Table 1 for details.

[0092] Among them, the flatness of the magnet is a deformation measurement index, which means taking the center point of the magnet as the zero point, and measuring the relative height data except the center point through tools such as height gauges, and measuring the maximum and minimum values ​​of the entire surface of the magnet. When the flatness is less than 0.25, it is a small deformation; when the flatness is 0.25-0.75, it is a medium deformation; when the flatness is greater than 0.75, it is a large deformation.

[0093] Table 1 Overall magnet flatness at different stages in Examples 1-6 and Comparative Examples 1-4 Examples and Comparative Examples Overall magnet flatness before diffusion bonding / mm Finally, the overall magnet flatness of the sample is obtained / mm Example 1 0.020 0.064 Example 2 0.022 0.089 Example 3 0.03 0.097 Example 4 0.005 0.021 Example 5 0.005 0.025 Example 6 0.005 0.036 Comparative Example 1 0.023 1.129 Comparative Example 2 0.006 0.466 Comparative Example 3 0.007 1.038 Comparative Example 4 0.006 0.497 Experimental analysis: from Figure 1 It can be seen that the Halbach array magnet assembly prepared by the grain boundary diffusion process is prone to deformation, and the single-piece magnets are also deformed, and the magnets can no longer fit tightly together. Figure 2 The state of the magnet assembly before and after deformation can also be seen.

[0094] It can be seen from Table 1 that, no matter the samples are obtained before diffusion bonding or after final processing, the overall magnet flatness of the samples in Examples 1-6 is better than that of the samples in Comparative Examples 1-4.

[0095] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for manufacturing a Halbach array magnet assembly, characterized in that: The steps include: 1) Preliminary processing of the blank material according to size requirements to obtain a permanent magnet blank; 2) Perform Halbach array arrangement and mark the bonding surface and non-bonding surface on the permanent magnet blank; 3) Coating an adhesive layer on the bonding surface of the permanent magnet blank, coating an anti-oxidation layer on the non-bonding surface of the magnet blank, bonding the bonding surfaces, and then performing diffusion bonding treatment under vacuum and pressure conditions to obtain a heat-treated component product; 4) Reprocess the heat-treated component products to meet the size requirements of the target Halbach array, forming a semi-finished Halbach array magnet component; 5) Surface processing of the semi-finished products of Halbach array magnet components; 6) Magnetizing the surface-processed semi-finished Halbach array magnet assembly according to the orientation direction to obtain the Halbach array magnet assembly; The thickness of the permanent magnet blank preliminarily processed in step 1) is not greater than 1.5 mm, and the aspect ratio is greater than 20.

2. The method for manufacturing the Halbach array magnet assembly according to claim 1, characterized in that: The thickness of the permanent magnet blank preliminarily processed in step 1) is 0.15-1.5 mm.

3. The method for manufacturing the Halbach array magnet assembly according to claim 1, characterized in that: In the step three, the thickness of the adhesive layer on the bonding surfaces between adjacent permanent magnet blanks is 0.3 μm-150 μm; the coating thickness on the non-bonding surfaces is 0.3 μm-200 μm.

4. The method for manufacturing the Halbach array magnet assembly according to claim 2, characterized in that: In the step three, the thickness of the adhesive layer on the bonding surfaces between adjacent permanent magnet blanks is 2.5 μm-25 μm; the coating thickness on the non-bonding surfaces is 14.5 μm-60 μm.

5. The method for manufacturing the Halbach array magnet assembly according to claim 1, characterized in that: The vacuum degree in step 3) is <1.0E-04, and the pressure is 2-30Mpa.

6. The method for manufacturing the Halbach array magnet assembly according to claim 1, characterized in that: In the step 3), the main component of the anti-oxidation layer coated on the non-bonding surface of the permanent magnet blank is metal powder and / or alloy powder, and / or the anti-oxidation layer is a high temperature resistant film layer; The main component of the adhesive layer coated on the bonding surface of the permanent magnet blank is metal powder and / or alloy powder.

7. The method for manufacturing the Halbach array magnet assembly according to claim 6, characterized in that: The metal element in the metal powder includes one of Tb, Dy, Gd, Ce, Pr, Nd, Al, Cu, Ag, Ni, Zn, Ga, Nb, Co, and Sn; the alloy powder is a low melting point rare earth alloy powder or is formed by at least two elements of Tb, Dy, Gd, Ce, Pr, Nd, Al, Cu, Ag, Ni, Zn, Ga, Nb, Co, Sn, and rare earth compounds; The composition of the low melting point rare earth alloy powder is RE-X, wherein RE is at least one of Tb, Dy, Pr, Nd, Gd, and Ce; X is at least one of Fe, Cu, Al, Ni, Sn, Nb, Ga, Ag, and Co; The high temperature resistant film layer includes a high temperature resistant metal film layer and a high temperature resistant ceramic film layer. The high temperature resistant metal film layer is deposited by a high melting point metal. The high melting point metal includes at least one of Ti, Cr, Ta, W, Mo, and V. The high temperature resistant ceramic film layer is a nitride or carbide ceramic film.

8. The method for manufacturing the Halbach array magnet assembly according to claim 6, characterized in that: The particle size of the metal powder and alloy powder used for coating on the non-bonding surface is 2-50 μm; the particle size of the metal powder and alloy powder used for coating on the bonding surface is 2-10 μm.

9. The method for manufacturing a Halbach array magnet assembly according to claim 6, wherein the coating liquid used when coating the adhesive layer is composed of metal powder and / or alloy powder and a solvent, and the solvent is at least one of anti-oxidation glue and ethanol; The coating liquid used when coating the anti-oxidation layer consists of metal powder and / or alloy powder and pinene alcohol.

Citation Information

Patent Citations

  • Integrated magnetizing method of Halbach array magnet assembly

    CN112530658A

  • Magnetic bodies spare that adopts bake array structure of haier and make up with ironbar

    CN205645427U

  • Halbach array magnet and manufacturing method thereof

    KR1020100036526A

  • Radiation calculation apparatus for nuclear power plant structures

    KR102608936B1

  • Magnetic field generator, method for manufacturing magnetic field generator, and linear motor using magnetic field generator

    US20220293320A1

Cited By

  • Linear Halbach array based on non-uniform permanent magnet and preparation method thereof

    CN120236849A

  • Welding pretreatment method and welding Halbach array magnetic assembly preparation method applied to welding pretreatment method

    CN122393127A