Method for improving radiation resistance of floating gate memory device

By using fluorine ion-doped SiO2 as the ONO medium in floating gate memory devices, the problem of threshold drift caused by radiation is solved, higher radiation resistance and device reliability are achieved, and oxide damage caused by reinforcement processing is avoided. .

CN118737829APending Publication Date: 2024-10-0158TH RES INST OF CETC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410664429.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Floating gate memory devices can easily cause threshold voltage drift in a radiation environment, leading to errors in stored information. Existing ion implantation reinforcement methods can damage the oxide and increase defects and reliability risks.

Method used

Fluorine ion-doped SiO2 is used as the ONO medium to replace traditional SiO2. The floating gate structure is formed by photolithography and CVD methods, which avoids reinforcement processing, reduces oxide damage, and improves radiation resistance.

Benefits of technology

Without damaging the oxide, the number of positive charges generated by ionizing radiation is reduced, the radiation resistance of the floating gate memory device is improved, the threshold drift is reduced, and the reliability of the device is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737829A_ABST
    Figure CN118737829A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving radiation resistance of a floating gate memory device, and belongs to the field of semiconductor process manufacturing. Firstly, a P-type substrate is provided, and an epitaxial silicon layer, a silicon dioxide layer and a barrier layer are sequentially formed on the P-type substrate; etching to form an STI silicon shallow slot, and growing SiO2 films on the side wall and the bottom of the STI silicon shallow slot in a thermal oxidation manner; then HDP medium filling is carried out on the STI by adopting a CVD method, then high-temperature annealing treatment is carried out, and the HDP medium is flattened; performing wet etching on the silicon dioxide layer and the barrier layer; gate oxide is grown through thermal oxidation, and floating gate polycrystal deposition is carried out by adopting a CVD (Chemical Vapor Deposition) method; performing dry etching on the gate oxide and the floating gate polycrystal; sequentially depositing a silicon dioxide layer, a silicon nitride layer and a silicon dioxide layer by adopting a CVD (Chemical Vapor Deposition) method to form an ONO dielectric film; carrying out control gate polycrystal deposition by adopting CVD (Chemical Vapor Deposition); performing dry etching on the ONO dielectric film and the control gate polycrystal; and finally carrying out lightly doped drain injection, side wall growth etching and source drain injection, wherein the subsequent process follows a universal CMOS (Complementary Metal-Oxide-Semiconductor Transistor) process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor process manufacturing, and in particular to a method for improving the radiation resistance performance of a floating gate storage device. Background Art

[0002] Floating gate memory devices mainly rely on the charge on the floating gate to store information. The ionizing radiation of high-energy protons, electrons and X-rays in the space radiation environment will change the polarity and quantity of the charge of the floating gate memory device, causing the threshold voltage of the floating gate memory device to drift, which in turn leads to errors in the storage information of the floating gate memory device.

[0003] The radiation effect of floating gate memory devices is closely related to the oxide around the floating gate, and the radiation response of the programming state and the erased state is different. For the floating gate memory device in the programming state, since the floating gate stores electrons, the floating gate potential is high, and the ionizing radiation generates electron-hole pairs in the ONO and the gate oxide, wherein the electrons drift to the substrate and the control gate under the action of the electric field, and part of the holes are captured by the traps in the gate oxide and the ONO, and the remaining holes are transported to the floating gate and recombined with the electrons stored on the floating gate, thereby reducing the number of electrons stored on the floating gate, and the threshold of the floating gate memory device is thus reduced; for the floating gate memory device in the erased state, since the floating gate stores holes, the floating gate potential is low, and the ionizing radiation generates electron-hole pairs in the ONO and the gate oxide, wherein the holes are captured by the traps in the gate oxide and the ONO, and the electrons drift to the floating gate under the action of the electric field and recombined with the holes stored on the floating gate, thereby reducing the number of holes in the floating gate memory device, and the threshold of the floating gate memory device is thus increased. Therefore, the impact of the oxide around the floating gate on the floating gate Flash is mainly reflected in lowering its programming state threshold and increasing its erase state threshold, thereby reducing the threshold window and causing read errors.

[0004] An effective way to improve the radiation resistance of floating gate memory devices is to introduce electron trap centers to recombine holes generated by ionizing radiation, thereby reducing the number of holes transported to the floating gate and improving the radiation resistance of floating gate memory devices. Patent CN104217925A uses the method of fluorine ion implantation to introduce electron trap centers, thereby reducing the density of trapped holes in the buried oxide layer in SOI materials.

[0005] However, the ion implantation reinforcement method will damage the oxide, causing an increase in defects in the oxide, thereby affecting device reliability. Summary of the invention

[0006] The object of the present invention is to provide a method for improving the radiation resistance of a floating gate memory device to solve the problems in the background technology.

[0007] In order to solve the above technical problems, the present invention provides a method for improving the radiation resistance of a floating gate memory device, comprising:

[0008] Step 1, providing a P-type substrate, and sequentially forming an epitaxial silicon layer, a silicon dioxide layer and a barrier layer on the P-type substrate;

[0009] Step 2, performing photolithography on the epitaxial silicon layer, etching away the barrier layer, the silicon dioxide layer and a portion of the epitaxial silicon layer in the exposure area in sequence, and etching to form a STI silicon shallow groove;

[0010] Step 3, filling the STI silicon shallow trench with HDP dielectric, then performing high temperature annealing, and finally planarizing the HDP dielectric;

[0011] Step 4, completely removing the silicon dioxide layer and the barrier layer;

[0012] Step 5: thermally oxidize and grow gate oxide, and then use CVD method to deposit floating gate polycrystalline;

[0013] Step 6, dry etching the gate oxide and floating gate polycrystalline;

[0014] Step 7, sequentially depositing a silicon dioxide layer, a silicon nitride layer, and a silicon dioxide layer to form an ONO dielectric film;

[0015] Step 8: using CVD to deposit control gate polycrystalline;

[0016] Step 9, dry etching the ONO dielectric film and control gate polycrystalline;

[0017] Step 10: Perform lightly doped drain implantation, sidewall growth etching, and source and drain implantation. Subsequent processes follow the general CMOS process.

[0018] In one embodiment, the resistivity of the P-type substrate is 8 to 12 Ω-cm; the resistivity of the epitaxial silicon layer is 8 to 12 Ω-cm, and the thickness is 6.0 to 7.0 μm.

[0019] In one embodiment, the barrier layer is a silicon nitride layer.

[0020] In one embodiment, the gate oxide is a SiO2 film grown by thermal oxidation, with a thickness of 8 to 10 nm.

[0021] In one embodiment, the silicon dioxide layer in the ONO medium is fluorosilicate glass.

[0022] In one embodiment, in step 3, the HDP dielectric is planarized, a portion of the barrier layer is polished as an over-removal, and the polishing stops on the barrier layer to ensure that no oxide layer remains on the barrier layer.

[0023] In one embodiment, in step 5, the floating gate poly covers the gate oxide and the HDP dielectric.

[0024] The present invention provides a method for improving the radiation resistance of a floating gate memory device. In the ONO growth step, fluorine ion-doped SiO2 (fluorosilicate) is used to replace traditional SiO2. The fluorine ion doping is more uniform, causing less damage to the oxide, without dielectric damage caused by ion bombardment, and without the need for additional reinforcement injection process, so the process difficulty and cost are lower. Since changing the gate oxygen doping will affect the programming and erasing mechanism of the floating gate memory device, the present invention does not perform reinforcement treatment on the gate oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a flowchart of a method for improving the radiation resistance of a floating gate memory device.

[0026] Figure 2 It is a schematic diagram of sequentially forming a silicon dioxide layer and a barrier layer on a P-type substrate;

[0027] Figure 3 is a schematic diagram of forming a STI silicon shallow trench;

[0028] Figure 4 It is a schematic diagram of HDP dielectric flattening;

[0029] Figure 5 is a schematic diagram of grinding a portion of the barrier layer as a process to remove and stop at the barrier layer;

[0030] Figure 6 is a schematic diagram of removing the silicon dioxide layer and the barrier layer by wet etching;

[0031] Figure 7 It is a schematic diagram of gate oxide growth and floating gate polycrystalline deposition;

[0032] Figure 8 It is a schematic diagram of using dry etching of gate oxide and floating gate polycrystalline;

[0033] Fig. 9 It is a schematic diagram of ONO dielectric film deposition;

[0034] Fig. 9A yes Fig. 9 A magnified schematic diagram of the A position (ONO dielectric film);

[0035] Fig.10 is a schematic diagram of control gate polycrystalline deposition;

[0036] Fig.11 It is a schematic diagram of dry etching of ONO dielectric film and control gate polycrystalline;

[0037] Fig.12 is a schematic diagram of forming a radiation-resistant floating gate memory device structure; DETAILED DESCRIPTION

[0038] The following is a further detailed description of a method for improving the radiation resistance of a floating gate memory device proposed by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0039] The present invention provides a method for improving the radiation resistance of a floating gate memory device, the process of which is as follows: Figure 1 As shown, the following steps are included:

[0040] like Figure 2 As shown, a P-type substrate 1 is provided, and an epitaxial silicon layer 2, a silicon dioxide layer 3 and a barrier layer 4 are sequentially formed on the P-type substrate 1. Further, the resistivity of the P-type substrate 1 is 8 to 12 Ω-cm; the resistivity of the epitaxial silicon layer 2 is 8 to 12 Ω-cm, and the thickness is 6.0 to 7.0 μm; further, the barrier layer 4 is a silicon nitride layer.

[0041] like Figure 3 As shown, the epitaxial silicon layer 2 is then photolithographically processed to sequentially etch away the barrier layer 4, the silicon dioxide layer 3 and a portion of the epitaxial silicon layer 2 in the exposure area to form a STI silicon shallow trench 5.

[0042] like Figure 4 As shown, the STI silicon shallow trench 5 is filled with HDP dielectric 6 by CVD method. Then the HDP dielectric 6 is subjected to high temperature annealing treatment; Figure 5 As shown, dielectric planarization is then performed, a portion of the barrier layer 4 is polished for removal, and the polishing stops on the barrier layer 4 to ensure that no oxide layer remains on the barrier layer 4.

[0043] Then, wet etching is used to completely remove the barrier layer 4 and the silicon dioxide layer 3 to form a Figure 6 The structure shown.

[0044] like Figure 7 As shown, the gate oxide 7 is then grown by thermal oxidation, and the floating gate polycrystalline 8 is deposited by a CVD method; the floating gate polycrystalline 8 covers the gate oxide 7 and the HDP dielectric 6 .

[0045] The gate oxide 7 is photolithographically processed, and the floating gate polycrystalline 8 and the gate oxide 7 are sequentially etched away by dry etching to form a Figure 8 The structure shown.

[0046] like Fig. 9 As shown, then, a silicon dioxide layer, a silicon nitride layer, and a silicon dioxide layer are sequentially deposited by a CVD method to form an ONO dielectric film 9. The specific structure of the ONO dielectric film 9 is shown in FIG. Fig. 9A As shown;

[0047] like Fig.10 As shown, the control gate polycrystalline 10 is deposited by a CVD method.

[0048] Next, the control gate polycrystalline 10 and the ONO dielectric film 9 are dry-etched to form Fig.11 The structure shown.

[0049] Finally, the technicians can follow the general CMOS process according to the knowledge in the field, and perform lightly doped drain implantation, sidewall 11 growth etching and source drain implantation as needed to finally form the following: Fig.12 The radiation-resistant floating gate memory device is shown.

[0050] Through the above process, fluorosilicate glass is used to replace traditional SiO2 as the ONO medium. The fluorosilicate glass reduces the amount of positive charges generated in the ONO medium by ionizing radiation, thereby reducing the threshold drift, so that the floating gate memory device has higher radiation resistance under the same radiation environment.

[0051] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for improving the radiation resistance of a floating gate memory device, characterized in that: include: Step 1, providing a P-type substrate, and sequentially forming an epitaxial silicon layer, a silicon dioxide layer and a barrier layer on the P-type substrate; Step 2, performing photolithography on the epitaxial silicon layer, etching away the barrier layer, the silicon dioxide layer and a portion of the epitaxial silicon layer in the exposure area in sequence, and etching to form a STI silicon shallow groove; Step 3, filling the STI silicon shallow trench with HDP dielectric, then performing high temperature annealing, and finally planarizing the HDP dielectric; Step 4, completely removing the silicon dioxide layer and the barrier layer; Step 5: thermally oxidize and grow gate oxide, and then use CVD method to deposit floating gate polycrystalline; Step 6, dry etching the gate oxide and floating gate polycrystalline; Step 7, sequentially depositing a silicon dioxide layer, a silicon nitride layer, and a silicon dioxide layer to form an ONO dielectric film; Step 8: using CVD to deposit control gate polycrystalline; Step 9, dry etching the ONO dielectric film and control gate polycrystalline; Step 10: Perform lightly doped drain implantation, sidewall growth etching, and source and drain implantation. Subsequent processes follow the general CMOS process.

2. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: The resistivity of the P-type substrate is 8-12Ω-cm; the resistivity of the epitaxial silicon layer is 8-12Ω-cm, and the thickness is 6.0-7.0μm.

3. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: The barrier layer is a silicon nitride layer.

4. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: The gate oxide is a SiO2 film grown by thermal oxidation, and has a thickness of 8-10 nm.

5. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: The silicon dioxide layer in the ONO medium is fluorosilicate glass.

6. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: In step 3, the HDP dielectric is planarized, a portion of the barrier layer is ground as an over-removal, and the grinding stops on the barrier layer to ensure that no oxide layer remains on the barrier layer.

7. The method for improving the radiation resistance of a floating gate memory device according to claim 1, characterized in that: In the step 5, the floating gate poly covers the gate oxide and the HDP dielectric.