Antimony selenide / antimony oxide barrier layer, antimony selenide photoelectric detector array and preparation method of antimony selenide / antimony oxide barrier layer and antimony selenide photoelectric detector array
By using vapor transport deposition and ultraviolet ozone treatment to form a P-N junction barrier layer in an antimony selenide photodetector array, the complexity and performance problems of traditional barrier layer preparation are solved, and the array performance and ease of preparation are significantly improved.
Patent Information
- Application Number
- CN202410759562.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
The preparation process of the barrier layer in the traditional antimony selenide photodetector array is complex, the uniformity and crystallinity of the film are poor, and high-temperature annealing can easily cause the antimony selenide film to decompose, affecting device performance.
The vapor transport deposition method is used to deposit antimony selenide on the surface of the N-type light-absorbing layer, and ultraviolet ozone treatment is performed on the surface of the P-type light-absorbing layer to form antimony oxide to form a P-N junction barrier layer, which simplifies the preparation process and suppresses crosstalk between pixels.
The performance of the antimony selenide photodetector array is significantly improved, the dark current is reduced, the preparation process is simplified, and the complexity and performance problems in the preparation of traditional barrier layers are solved.
Smart Images

Figure CN118738071A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of light detection technology, and in particular, relates to an antimony selenide / antimony oxide barrier layer and a preparation method thereof, and an antimony selenide photoelectric detector array and a preparation method thereof. Background Art
[0002] Antimony selenide (Sb2Se3) is an important semiconductor material. In recent years, it has attracted widespread attention in the field of optoelectronics, especially in the field of thin-film photodetectors. Due to its physical and chemical properties, antimony selenide has become a popular research material for efficient energy conversion devices such as photodetectors. With the development of antimony selenide photodetectors, how to integrate photodetectors into photodetector arrays has become a difficult problem that needs to be solved. The main problem is that there will be photoelectric crosstalk between the pixels of the photodetector. At this time, the crosstalk between the device pixels can be reduced by constructing a Schottky junction or a PN junction.
[0003] At present, the basic structure of antimony selenide photodetectors includes: substrate, bottom electrode, N-type light absorbing layer, P-type light absorbing layer, and top electrode. If a photodetector array is to be prepared, a barrier layer needs to be prepared on the P-type light absorbing layer to suppress current crosstalk. However, the traditional barrier layer preparation method has the following problems: (1) The traditional barrier layer requires multiple layers of thin films to be superimposed on the light absorbing layer, and the preparation process is complicated; (2) The traditional barrier layer is generally prepared by spin coating, and the uniformity and crystallinity of the prepared film are poor, and it is not conducive to large-scale production; (3) After the traditional barrier layer is prepared, high-temperature annealing is required to make the barrier layer film recrystallize, which is easy to cause the decomposition of the antimony selenide film, thereby deteriorating the device performance. Summary of the invention
[0004] The present invention focuses on solving the technical problems existing in the preparation of traditional barrier layers, and provides an antimony selenide / antimony oxide barrier layer and an antimony selenide photodetector array and a preparation method thereof. The PN junction barrier layer formed by the present invention can suppress the crosstalk between the pixels of the antimony selenide photodetector array, while reducing the dark current of each pixel, thereby significantly improving the performance of the detector array. The preparation process is simple, and provides a simple and effective solution for the vacuum method preparation of antimony selenide photodetector arrays.
[0005] In order to achieve the above-mentioned object of the invention, the present invention is implemented by the following technical solutions:
[0006] According to a first aspect of the present invention, a method for preparing an antimony selenide / antimony oxide barrier layer is provided, comprising: using a vapor transport deposition method to deposit antimony selenide as a P-type light absorbing layer on the surface of an N-type light absorbing layer, performing ultraviolet ozone treatment on the surface of the P-type light absorbing layer to form antimony oxide, and the antimony oxide and the surface of the P-type light absorbing layer together constitute a PN junction barrier layer.
[0007] Preferably, the deposition temperature of the P-type light absorbing layer is 500-560° C., and the deposition time is 1-2 min.
[0008] Preferably, the temperature of the ultraviolet ozone treatment is 25-50° C., and the time is 15-30 minutes.
[0009] According to a second aspect of the present invention, there is provided an antimony selenide / antimony oxide barrier layer obtained by the above preparation method.
[0010] According to a third aspect of the present invention, an antimony selenide photodetector array is provided, comprising a PN junction barrier layer, wherein the PN junction barrier layer is the above-mentioned antimony selenide / antimony oxide barrier layer.
[0011] Furthermore, the antimony selenide photodetector array includes a substrate, a bottom electrode, an N-type light absorbing layer, a P-type light absorbing layer, a PN junction barrier layer and a top electrode which are stacked in sequence.
[0012] Preferably, the material of the substrate is soda-lime glass, sodium-free glass or quartz glass.
[0013] Preferably, the thickness of the bottom electrode is 100-200 nm; and the material of the bottom electrode is ITO.
[0014] Preferably, the thickness of the N-type light absorbing layer is 20-60 nm; the material of the N-type light absorbing layer is ZnO, SnO2 or TiO2.
[0015] Preferably, before the ultraviolet ozone treatment, the thickness of the P-type light absorbing layer is 300-1500 nm.
[0016] Preferably, after the ultraviolet ozone treatment, the thickness of the PN junction barrier layer is 1-10 nm.
[0017] Preferably, the thickness of the top electrode is 40-80 nm; and the material of the top electrode is Au or Ag.
[0018] According to a fourth aspect of the present invention, there is provided a method for preparing the antimony selenide photodetector array, comprising:
[0019] forming a bottom electrode on the substrate;
[0020] forming an N-type light absorbing layer on the bottom electrode;
[0021] Antimony selenide is deposited on the surface of the N-type light absorbing layer as a P-type light absorbing layer by using a vapor transport deposition method;
[0022] Performing ultraviolet ozone treatment on the surface of the P-type light absorbing layer to form antimony oxide, wherein the antimony oxide and the surface of the P-type light absorbing layer together constitute a PN junction barrier layer;
[0023] A top electrode is formed on the PN junction barrier layer.
[0024] The beneficial effects of the present invention are:
[0025] The present invention uses ultraviolet ozone to treat the surface of the P-type light-absorbing layer of antimony selenide, oxidizes the surface of the P-type light-absorbing layer of antimony selenide to generate antimony oxide, thereby preparing a PN junction barrier layer of antimony selenide / antimony oxide, and the PN junction barrier layer can suppress the crosstalk between each pixel point of the detector array, significantly improving the performance of the detector array. The present invention has a simple process, effectively solves the crosstalk problem between each pixel point of the photodetector array, and provides a simple and effective solution for preparing an antimony selenide photodetector array by a vacuum method. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope of the present invention.
[0027] Figure 1 Surface Raman test images of the P-type light absorbing layer obtained in Example 1 and Comparative Example 1.
[0028] Figure 2 This is a schematic diagram of the structure of the antimony selenide photodetector array prepared in Example 2.
[0029] Figure 3 The IV curves of the antimony selenide photodetector array prepared under different UV-ozone treatment times.
[0030] Figure 4 The IV curve of the antimony selenide photodetector array prepared under different P-type absorption layer deposition times.
[0031] Figure 5 3 and 4. The current distribution diagram of the antimony selenide photodetector array obtained in Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0032] The following is a more detailed description of the specific implementation of the present invention in conjunction with the accompanying drawings and embodiments, so as to better understand the scheme of the present invention and its advantages in various aspects. It should be noted that the specific implementation methods and embodiments described below are only for the purpose of illustration, and are not intended to limit the present invention.
[0033] The present invention provides an antimony selenide / antimony oxide barrier layer and a preparation method thereof, specifically, using a vapor transport deposition method to deposit antimony selenide on the surface of an N-type light absorbing layer as a P-type light absorbing layer, performing ultraviolet ozone treatment on the surface of the P-type light absorbing layer to form antimony oxide, and the antimony oxide and the surface of the P-type light absorbing layer together constitute a PN junction barrier layer.
[0034] As a preferred implementation, the deposition temperature of the P-type light absorbing layer is 500-560° C., and the deposition time is 1-2 min.
[0035] As a preferred embodiment, the temperature of the ultraviolet ozone treatment is 25 to 50° C., and the time is 15 to 30 minutes.
[0036] Furthermore, the present invention provides an antimony selenide photodetector array, wherein the PN junction barrier layer of the antimony selenide photodetector array is the above-mentioned antimony selenide / antimony oxide barrier layer.
[0037] Furthermore, the antimony selenide photodetector array includes a substrate, a bottom electrode, an N-type light absorbing layer, a P-type light absorbing layer, a PN junction barrier layer and a top electrode which are stacked in sequence.
[0038] As a preferred embodiment, the material of the substrate is soda-lime glass, soda-free glass or quartz glass.
[0039] As a preferred implementation, the thickness of the bottom electrode is 100-200 nm; the material of the bottom electrode is ITO.
[0040] As a preferred implementation, the thickness of the N-type light absorbing layer is 20-60 nm; the material of the N-type light absorbing layer is ZnO, SnO2 or TiO2.
[0041] As a preferred embodiment, before the ultraviolet ozone treatment, the thickness of the P-type light absorbing layer is 300-1500 nm.
[0042] As a preferred implementation, after the ultraviolet ozone treatment, the thickness of the PN junction barrier layer is 1-10 nm.
[0043] As a preferred implementation, the thickness of the top electrode is 40-80 nm; the material of the top electrode is Au or Ag.
[0044] Furthermore, the present invention provides a method for preparing an antimony selenide photodetector array, comprising:
[0045] forming a bottom electrode on the substrate;
[0046] forming an N-type light absorbing layer on the bottom electrode;
[0047] Antimony selenide is deposited on the surface of the N-type light absorbing layer as a P-type light absorbing layer by using a vapor transport deposition method;
[0048] Performing ultraviolet ozone treatment on the surface of the P-type light absorbing layer to form antimony oxide, wherein the antimony oxide and the surface of the P-type light absorbing layer together constitute a PN junction barrier layer;
[0049] A top electrode is formed on the PN junction barrier layer.
[0050] Example 1
[0051] A method for preparing an antimony selenide / antimony oxide barrier layer comprises the following steps:
[0052] Antimony selenide is deposited on the N-type light absorbing layer using vapor transport deposition method as a P-type light absorbing layer. The deposition temperature of the P-type light absorbing layer is 530°C and the deposition time is 1 min. The surface of the P-type light absorbing layer is treated with ultraviolet ozone at a treatment temperature of 25°C and a treatment time of 15 min.
[0053] Comparative Example 1
[0054] Antimony selenide is deposited on the N-type light-absorbing layer using vapor transport deposition as the P-type light-absorbing layer of the detector. The deposition temperature of the P-type light-absorbing layer is 530° C. and the deposition time is 1 min.
[0055] Effect verification 1: Raman test
[0056] In order to explore the substances generated on the surface of the P-type light absorbing layer after the UV-ozone treatment, Raman spectroscopy tests were performed on the P-type light absorbing layer treated with UV-ozone in Example 1 and the P-type light absorbing layer not treated with UV-ozone in Comparative Example 1, respectively: Figure 1 As shown, it can be seen from the Raman spectrum measurement results that antimony oxide peaks appear in the P-type light-absorbing layer after UV ozone treatment, proving that antimony oxide is generated on the surface of the P-type light-absorbing layer, that is, the preparation of antimony selenide / antimony oxide PN junction barrier layer is achieved.
[0057] Example 2
[0058] like Figure 2 As shown, a method for preparing an antimony selenide photodetector array comprises the following steps:
[0059] 1. ZnO was prepared as an N-type light absorbing layer on the bottom electrode by magnetron sputtering method. The thickness of the N-type light absorbing layer was 30 nm.
[0060] 2. Antimony selenide is deposited on the N-type light absorbing layer using vapor transport deposition as a P-type light absorbing layer. The deposition temperature of the P-type light absorbing layer is 530°C and the deposition time is 2 minutes. UV ozone treatment is performed on the surface of the P-type light absorbing layer at a treatment temperature of 25°C and a treatment time of 15 minutes.
[0061] 3. A 60 nm thick gold layer was prepared on the barrier layer as the top electrode by evaporation method.
[0062] Example 3
[0063] The only difference from Example 2 is that no ultraviolet ozone treatment is performed.
[0064] Example 4
[0065] The difference from Example 2 is that the ultraviolet ozone treatment time is changed to 30 minutes.
[0066] Effect Verification 2: Current-Voltage (IV) Test
[0067] The positive and negative electrodes of the antimony selenide photodetector arrays prepared in Examples 2, 3 and 4 were connected to the IV test module of the semiconductor analyzer. 2 The voltage-current curve of the detector array is obtained by irradiating the detector array under light intensity.
[0068] The test results are as follows Figure 3 As shown by Figure 3 It can be seen that the photocurrent of the antimony selenide photodetector array that is not treated with ultraviolet ozone cannot be suppressed at -1V~1V, and the current can flow normally; the photocurrent of the antimony selenide photodetector array that has been treated with ultraviolet ozone can be effectively suppressed at -1V~1V, achieving a barrier effect.
[0069] It can be seen that the ultraviolet ozone treatment of the present invention for 15 to 30 minutes is a more preferred treatment time, and the thickness of the PN junction barrier layer obtained after the treatment is generally 1 to 10 nm; the ultraviolet ozone treatment temperature of the present invention is generally 25 to 50°C.
[0070] Example 5
[0071] The only difference from Example 2 is that the deposition time of the P-type light absorbing layer is 1 minute.
[0072] Example 6
[0073] The only difference from Example 2 is that the deposition time of the P-type light absorbing layer is 3 minutes.
[0074] Effect Verification 3: Current-Voltage (IV) Test
[0075] The positive and negative electrodes of the antimony selenide photodetector arrays prepared in Examples 2, 5 and 6 were connected to the IV test module of the semiconductor analyzer. 2 The voltage-current curve of the detector array is obtained by irradiating the detector array under light intensity.
[0076] The test results are as follows Figure 4 As shown by Figure 4It can be seen that different deposition times of the P-type light absorbing layer have an impact on the detector array current. If the deposition time is too long, the thickness of the P-type light absorbing layer will be thicker and the series resistance will increase.
[0077] Therefore, the present invention selects a deposition temperature of 500-560° C. and a deposition time of 1-2 min as the preferred preparation conditions for the P-type light absorbing layer; the thickness of the P-type light absorbing layer obtained by vapor transport deposition is 300-1500 nm, which is a better effect.
[0078] Comparative Example 2
[0079] 1. ZnO was prepared as an N-type light absorbing layer on the bottom electrode by magnetron sputtering method. The thickness of the N-type light absorbing layer was 30 nm.
[0080] 2. Antimony selenide is deposited on the N-type light absorbing layer using a vapor transport deposition method as a P-type light absorbing layer. The deposition temperature of the P-type light absorbing layer is 530°C and the deposition time is 2 minutes.
[0081] 3. A 60nm thick gold layer was prepared on the P-type light-absorbing layer by evaporation method as the top electrode.
[0082] Effect Verification 2: Current-Time (IT) Test
[0083] The positive and negative electrodes of the antimony selenide photodetector arrays prepared in Test Example 2 and Comparative Example 2 were connected to the IT test module of a semiconductor analyzer to measure the current value of each pixel in the array.
[0084] The test results are as follows Figure 5 As shown by Figure 5 It can be seen that compared with the detector array without a barrier layer prepared in Comparative Example 2, the detector array with a barrier layer prepared in Example 2 can suppress the current crosstalk between each pixel point of the detector array due to the presence of the barrier layer, thereby significantly improving the performance of the detector array.
[0085] Although the preferred embodiments of the present invention have been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms of specific changes without departing from the scope of protection of the invention and the claims, all of which fall within the scope of protection of the present invention.
Claims
1. A method for preparing an antimony selenide / antimony oxide barrier layer, characterized in that: include: Antimony selenide is deposited on the surface of the N-type light absorbing layer as a P-type light absorbing layer by using a vapor transport deposition method, and the surface of the P-type light absorbing layer is treated with ultraviolet ozone to form antimony oxide, which together with the surface of the P-type light absorbing layer constitutes a PN junction barrier layer.
2. The method for preparing an antimony selenide / antimony oxide barrier layer according to claim 1, characterized in that: The deposition temperature of the P-type light absorbing layer is 500-560° C., and the deposition time is 1-2 minutes.
3. The method for preparing an antimony selenide / antimony oxide barrier layer according to claim 1, characterized in that: The temperature of the ultraviolet ozone treatment is 25-50° C., and the time is 15-30 minutes.
4. An antimony selenide / antimony oxide barrier layer, characterized in that: The method is obtained by the preparation method described in any one of claims 1 to 3.
5. An antimony selenide photodetector array, comprising a PN junction barrier layer, characterized in that: The PN junction barrier layer is the antimony selenide / antimony oxide barrier layer as described in claim 4.
6. The antimony selenide photodetector array according to claim 5, characterized in that: The invention comprises a substrate, a bottom electrode, an N-type light absorbing layer, a P-type light absorbing layer, a PN junction barrier layer and a top electrode which are stacked in sequence.
7. The antimony selenide photodetector array according to claim 6, characterized in that: The thickness of the bottom electrode is 100-200 nm; The thickness of the N-type light absorbing layer is 20 to 60 nm; Before the ultraviolet ozone treatment, the thickness of the P-type light absorbing layer is 300 to 1500 nm; After the ultraviolet ozone treatment, the thickness of the PN junction barrier layer is 1 to 10 nm; The thickness of the top electrode is 40-80 nm.
8. The antimony selenide photodetector array according to claim 5, characterized in that: The material of the substrate is soda-lime glass, sodium-free glass or quartz glass, the material of the bottom electrode is ITO, the material of the N-type light-absorbing layer is ZnO, SnO2 or TiO2, and the material of the top electrode is Au or Ag.
9. A method for preparing an antimony selenide photodetector array according to any one of claims 6 to 8, characterized in that: include: forming a bottom electrode on the substrate; forming an N-type light absorbing layer on the bottom electrode; Antimony selenide is deposited on the surface of the N-type light absorbing layer as a P-type light absorbing layer by using a vapor transport deposition method; Performing ultraviolet ozone treatment on the surface of the P-type light absorbing layer to form antimony oxide, wherein the antimony oxide and the surface of the P-type light absorbing layer together constitute a PN junction barrier layer; A top electrode is formed on the PN junction barrier layer.