Solar cell buffer layer and preparation method thereof
By regulating the composition of the CdZn(O,S) film in the solar cell, the problem of poor composition of the Zn(O,S) film in the existing technology is solved, the matching with the CIGS absorption layer and the efficiency of the solar cell are improved, and the efficiency of the solar cell is reduced. production costs.
Patent Information
- Application Number
- CN202310326961.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
The proportion of S element in the Zn(O,S) thin film material composition prepared by the existing chemical water bath deposition process is too low, and the composition control range is narrow, resulting in a completely cadmium-free Zn(O,S) buffer layer and CIGS absorption layer in the lattice and band. Poor performance in gap matching affects solar cell efficiency.
By placing the growth substrate into contact with a mixture containing a cadmium source, a zinc source, a complexing agent, a sulfur source and a pH adjuster, the concentration of the cadmium source and the molar ratio of the zinc source to the cadmium source are controlled to regulate Cd/(Zn+Cd ) and S/(S+O) ratio, prepare high-quality CdZn(O,S) thin films, expand their composition and band gap adjustment range, and improve the matching with the CIGS absorption layer.
A CdZn(O,S) thin film with good optical transparency and electrical conductivity was obtained, which significantly improved the matching between the thin film buffer layer and the CIGS absorption layer, improved solar cell efficiency, and reduced production costs and waste treatment burden.
Smart Images

Figure BDA0004153599610000071 
Figure BDA0004153599610000081 
Figure HDA0004153599620000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a solar cell buffer layer and a preparation method thereof. Background Art
[0002] In the laboratory or industrial process steps of mainstream CIGS thin-film solar cells, a chemical water bath is usually used to prepare a buffer layer film using a reaction precursor solution. At a certain temperature, the particles undergo nucleation and growth to react on the substrate to form a buffer layer film. The cadmium-free Zn(O,S) film obtained by chemical water bath deposition is a mixture of ZnS, ZnO and Zn(OH)2. The band gap Eg of Zn(O,S) is adjustable from 2.8 to 3.8 eV depending on the S content. The sulfur ratio at the minimum band gap is 0.7, which enhances its ability to collect short-wave visible light and has a higher light transmittance than CdS. The lattice constant of Zn(O,S) is linearly related to the S component, and the band edge position of Zn(O,S) will also change with the change of S content. Therefore, the band gap width, lattice constant and band edge position of Zn(O,S) are closely related to the composition.
[0003] Although wide bandgap and cadmium-free Zn(O,S) is considered to be the most promising next-generation buffer material to replace CdS and quickly realize industrial application. However, the proportion of S element in the Zn(O,S) thin film material prepared by chemical water bath is too low and the composition control range is narrow, which has poor lattice and bandgap matching with CIGS absorption layer, resulting in the efficiency of CIGS thin film solar cells with cadmium-free Zn(O,S) buffer layer always being lower than that of CdS buffer layer cells. Therefore, the development of CdZn(O,S) quaternary compound semiconductor thin film materials came into being.
[0004] At present, the process of chemical water bath deposition of CdZn(O,S) thin films generally has the following problems: 1) The amount of cadmium salt used in the preparation process is large, and the burden of waste liquid treatment is heavy; 2) The quality of the deposited film is poor, and there are many hole-like defects; 3) The photoelectric properties of the prepared film are not good; 4) The film and the CIGS absorption layer have poor lattice and band gap matching. Summary of the invention
[0005] In view of this, the main purpose of the present application is to provide a solar cell buffer layer and a preparation method thereof, wherein the obtained CdZn (O, S) thin film has good surface quality, excellent optical transparency and conductivity, and the CdZn (O, S) thin film lattice and band gap are adjustable, thereby improving the matching degree between the thin film buffer layer and the CIGS absorption layer.
[0006] To achieve the above-mentioned purpose of the invention, the first aspect of the present application provides a solar cell buffer layer, wherein the solar cell buffer layer is a CdZn(O,S) thin film, wherein the Cd / (Zn+Cd) ratio ranges from 0.03-0.94, and the S(S+O) ratio ranges from 0.36-0.74.
[0007] Furthermore, the Cd / (Zn+Cd) ratio ranges from 0.03 to 0.81.
[0008] A second aspect of the present invention provides a method for preparing a buffer layer for a solar cell, the method comprising:
[0009] placing the growth substrate in a mixed solution comprising a cadmium source, a zinc source, a complexing agent, a sulfur source and a pH adjuster for contact;
[0010] Wherein, in the mixed solution, the molar ratio of the cadmium source to the zinc source is (0.001-0.1):1, the concentration of the cadmium source is 0.045mmol / L-4.5mmol / L, and the pH value of the mixed solution is 10.3-11.
[0011] Furthermore, the molar ratio of the cadmium source, the zinc source, the complexing agent and the sulfur source is (0.001-0.1):1:(0.75-1.25):(3-8).
[0012] Furthermore, the contact conditions include a contact temperature of 75-90° C. and a contact time of 10-40 min.
[0013] Furthermore, the zinc source is selected from at least one of zinc nitrate, zinc acetate, zinc oxalate, zinc sulfate and zinc chloride.
[0014] Furthermore, the cadmium source is selected from at least one of cadmium nitrate, cadmium acetate, cadmium oxalate, cadmium sulfate and cadmium chloride.
[0015] Furthermore, the complexing agent is selected from at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, nitrilotriacetic acid, trisodium nitrilotriacetate, and triethanolamine.
[0016] Furthermore, the sulfur source is selected from at least one of thiourea, thioacetamide and sodium thiosulfate.
[0017] Furthermore, the pH regulator is selected from at least one of sodium hydroxide, ammonia water, hydrazine and hydrazine.
[0018] The third aspect of the present application provides a solar cell buffer layer prepared by the above preparation method.
[0019] Compared with the prior art, this application has the following advantages:
[0020] According to the method provided by the present application, the growth substrate is placed in a mixed solution containing a cadmium source, a zinc source, a complexing agent, a sulfur source and a pH regulator for contact. In this process, an appropriate amount of Cd doping is introduced to generate defect energy levels and increase the carrier concentration, thereby obtaining a high-quality CdZn (O, S) film with excellent optical transparency and conductivity. At the same time, the present invention controls the composition, band gap and microstructure of the CdZn (O, S) film by controlling the cadmium source concentration and changing the molar ratio of the zinc source to the cadmium source in the mixed solution. The prepared CdZn (O, S) film composition control range is significantly expanded, and the film lattice and band gap adjustment range are expanded, so that it can be applied to CIGS absorption layers with different band gaps, which is beneficial to improve the matching of the interface between the buffer layer and the absorption layer of the thin-film solar cell.
[0021] Other features and advantages of the present application will be described in detail through the following specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1-2 This is a scanning electron microscope image of the CdZn(O,S) film prepared in Example 1.
[0023] Figure 3-4 This is a scanning electron microscope image of the CdZn(O,S) film prepared in Example 2.
[0024] Figure 5-6 This is a scanning electron microscope image of the CdZn(O,S) thin film prepared in Example 3.
[0025] Figure 7-8 This is a scanning electron microscope image of the CdZn(O,S) film prepared in Example 4.
[0026] Fig. 9 Schematic diagram of transmittance test results of CdZn (O, S) films prepared in Examples 1-4 and Comparative Example 1.
[0027] Fig.10 Schematic diagram of reflectivity test results of CdZn (O, S) films prepared in Examples 1-4 and Comparative Example 1.
[0028] Fig.11 Schematic diagram of XPS test results of CdZn(O,S) films prepared in Examples 1-4 and Comparative Example 1. The numbers in the figure are the molar concentration ratios of the cadmium source and the zinc source. DETAILED DESCRIPTION
[0029] The present application is further described below in conjunction with embodiments, but the present application is not limited to the listed embodiments, but also includes equivalent improvements and modifications of the technical solutions defined in the claims attached to the present application.
[0030] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0031] In the following examples and comparative examples:
[0032] (1) Main raw materials
[0033] Unless otherwise specified, the raw materials involved in the examples of this application can be obtained from commercial channels.
[0034] (2) Characterization and testing
[0035] The films prepared in the embodiments and comparative examples were analyzed using a Nova Nano450 scanning electron microscope from FEI, and the thickness data of the films were measured by measuring the cross-sectional view of the SEM. The transmittance of the prepared solar cell buffer layer was tested in the wavelength range of 240-2400 using an ultraviolet-visible near-infrared spectrophotometer (UV-NIR) (UV3600 from Shimadzu, Japan), and the weighted average transmittance was calculated in the spectral range of 350-1300nm, and the optical band gap of the film was obtained by linear fitting of the absorption edge in the sample transmission spectrum. The S (S+O) in some CdZn (O, S) films was tested and calculated using an Escalab250Xi X-ray photoelectron spectrometer, where the test conditions included the excitation source being monochromatized Al Kα (1486.6eV) and the power being 300W.
[0036] A first aspect of the present invention provides a solar cell buffer layer, wherein the solar cell buffer layer is a CdZn(O,S) thin film, wherein the Cd / (Zn+Cd) ratio ranges from 0.03 to 0.94, and the S(S+O) ratio ranges from 0.36 to 0.74.
[0037] Furthermore, the Cd / (Zn+Cd) ratio ranges from 0.03 to 0.81.
[0038] The CdZn(O,S) film of the present invention includes a mixture of CdS, CdO, ZnS, and ZnO. The Cd / (Zn+Cd) ratio refers to the percentage of the number of atoms of the Cd element in the film to the sum of the number of atoms of the Cd element and the Zn element, and the S(S+O) ratio refers to the percentage of the number of atoms of the sulfur element in the film to the sum of the number of atoms of the sulfur element and the oxygen element.
[0039] A second aspect of the present invention provides a method for preparing a buffer layer for a solar cell, the method comprising:
[0040] placing the growth substrate in a mixed solution of a cadmium source, a zinc source, a complexing agent, a sulfur source and a pH adjuster for contact;
[0041] Wherein, in the mixed solution, the molar ratio of the cadmium source to the zinc source is (0.001-0.1):1, the concentration of the cadmium source is 0.045mmol / L-4.5mmol / L, and the pH value of the mixed solution is 10.3-11.
[0042] The growth substrate in the present invention is a CIGS absorption layer, which is not particularly limited, and any CIGS absorption layer commonly used in the art can be used in the present invention. The concentration of the cadmium source is measured by the molar concentration of the cadmium element contained in the cadmium source, the concentration of the zinc source is measured by the molar concentration of the zinc element contained in the zinc source, the concentration of the sulfur source is measured by the molar concentration of the sulfur element contained in the sulfur source, and the concentration of the complexing agent is measured by the molar concentration of the complexing agent itself.
[0043] The inventor of the present invention has found through research that during the contact process, the mixed solution is subjected to a chemical water bath deposition reaction on the surface of the growth substrate to prepare a CdZn(O,S) thin film, whose bandgap width, lattice constant and band edge position are closely related to the components. By doping a trace amount of cadmium elements and accurately controlling the concentration of the cadmium source in the mixed solution and its ratio to the zinc source, the ratio of Cd / (Zn+Cd) and S / (S+O) in the film composition can be effectively regulated, and the film lattice and band gap adjustment range can be expanded, so that it can be applied to CIGS absorption layers with different band gaps, and the matching of the interface between the buffer layer and the absorption layer of the thin film solar cell can be improved.
[0044] Furthermore, the molar ratio of the cadmium source, the zinc source, the complexing agent and the sulfur source is (0.001-0.1):1:(0.75-1.25):(3-8).
[0045] In a specific embodiment, the molar ratio of the cadmium source to the zinc source in the mixed solution can be 0.1, 0.01, 0.002, or 0.001.
[0046] The concentration of the cadmium source can be 4.5 mmol / L, 0.45 mmol / L, 0.09 mmol / L, or 0.045 mmol / L.
[0047] The concentration of the zinc source may be 0.03 mol / L, 0.045 mol / L, 0.06 mol / L, 0.075 mol / L, or 0.09 mol / L.
[0048] The pH value of the mixed solution can be 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9 and 11.
[0049] The molar concentration of the complexing agent can be 0.03 mol / L, 0.045 mol / L, 0.06 mol / L, 0.075 mol / L, or 0.09 mol / L.
[0050] The molar concentration of the sulfur source can be 0.05 mol / L, 0.15 mol / L, 0.3 mol / L, or 0.6 mol / L.
[0051] The sulfur source is in excess in the reaction solution, at a higher concentration than the zinc.
[0052] Any cadmium source that can be used in the art to prepare a buffer layer for a thin-film solar cell can be used in the present invention; in a specific embodiment, the cadmium source can be selected from at least one of cadmium nitrate, cadmium acetate, cadmium oxalate, cadmium sulfate and cadmium chloride, preferably cadmium sulfate.
[0053] All zinc sources that can be used in the art to prepare a buffer layer for a thin-film solar cell can be used in the present invention; in a specific embodiment, the zinc source can be selected from at least one of zinc nitrate, zinc acetate, zinc oxalate, zinc sulfate and zinc chloride, preferably zinc sulfate.
[0054] In a specific embodiment, the complexing agent is selected from at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, nitrilotriacetic acid, trisodium nitrilotriacetate, and triethanolamine, preferably sodium citrate. The complexing agent plays the role of complexing metal ions, controlling the reaction speed, and improving the film quality in the reaction.
[0055] Among them, sodium citrate refers to the sodium salt of citric acid, which can be trisodium citrate or disodium citrate. Sodium tartrate refers to the sodium salt of tartaric acid, which can be monosodium tartaric acid or disodium tartrate.
[0056] Any sulfur source that can be used in the art to prepare a buffer layer for a thin-film solar cell can be used in the present invention. Specifically, the sulfur source is selected from at least one of thiourea, thioacetamide, and sodium thiosulfate, preferably thiourea. The sulfur source provides S 2- , changes in sulfur source concentration will affect the reaction rate, film quality, film thickness and film transmittance.
[0057] In a specific embodiment, the pH regulator is selected from at least one of sodium hydroxide, ammonia, hydrazine, and hydrazine, preferably ammonia. Ammonia can release OH - , promoting the hydrolysis of thiourea to generate S 2- On the one hand, ammonia water acts as a pH regulator. On the other hand, since ammonia water is also a complexing agent, its complexing ability is lower than that of complexing agents such as trisodium citrate.
[0058] The pH value of the mixed solution mainly affects the degree of hydrolysis of thiourea. In the present invention, due to the addition of the complexing agent, the pH regulator is mainly used to adjust the pH value of the mixed solution.
[0059] The present invention does not specifically limit the configuration of the mixed solution, and any common method in the art can be used in the present invention. In a preferred embodiment, the method for configuring the mixed solution includes respectively adding a cadmium source, a zinc source and a complexing agent to a sulfur source, dissolving and mixing them uniformly, and then adding a pH regulator and mixing them thoroughly.
[0060] The present invention has no particular limitation on the solvents for the cadmium source, zinc source, complexing agent and sulfur source, as long as the substances can be fully dissolved.
[0061] In a specific embodiment, the contact conditions include a contact temperature of 75-90° C., more preferably 80-85° C., and a contact time of 10-40 min, more preferably 20-30 min. The above contact conditions are conducive to obtaining a film with suitable thickness, transmittance and high surface quality.
[0062] Among them, the contact temperature can be 80℃, 81℃, 82℃, 83℃, 84℃, 85℃, 86℃, 87℃, 89℃, and 90℃.
[0063] Those skilled in the art will appreciate that, in order to obtain a thin-film solar cell buffer layer with better surface quality on the growth substrate, the growth substrate may be placed in an organic solvent and deionized water for ultrasonic cleaning in sequence before being placed in the mixed solution.
[0064] The present invention does not specifically limit the cleaning of the growth substrate, and the organic solvents and cleaning conditions commonly used in the art can be used in the present invention.
[0065] In a preferred embodiment, during the contacting, the mixed liquid can be poured into the reaction container so that the growth substrate is immersed to a certain depth below the liquid surface of the mixed liquid.
[0066] In a preferred embodiment, after the contact is completed, the growth substrate is taken out and cleaned and dried. The present invention does not specifically limit the cleaning and drying, and conventional operations in the art can be used. Drying is preferably carried out by blowing with nitrogen.
[0067] The inventors have found through research that by using the preparation method of the present invention to prepare a solar cell buffer layer, a high-quality thin film product can be obtained after the growth substrate is removed from the mixed liquid, cleaned and dried with nitrogen. The thin film is evenly covered on the surface of the growth substrate, has no cracks or holes, and can be directly used as a buffer layer in the device structure of a thin-film solar cell without further surface treatment. It is highly compatible with existing CdS water bath deposition equipment, and does not require additional process steps and equipment in large-scale production.
[0068] The following embodiments are used to illustrate the solar cell buffer layer and the preparation method thereof of the present invention.
[0069] Example 1
[0070] 1) The CIGS absorption layer used as the growth substrate is cleaned in an organic solvent and clean water respectively.
[0071] 2) Mix cadmium sulfate and zinc sulfate solutions of different concentrations and proportions with trisodium citrate solution, add 25% ammonia water by mass, increase the amount of ammonia water according to the real-time monitoring value of pH, and then add thiourea solution. The final pH value of the solution is 10.5.
[0072] In the obtained mixed solution, the concentration of cadmium sulfate is 4.5mmol / L, the concentration of zinc sulfate is 0.045mol / L, the concentration of trisodium citrate is 0.045mol / L, the concentration of thiourea is 0.15mol / L, and the pH value of the mixed solution is 10.5. Therefore, the molar ratio of the cadmium source to the zinc source in the mixed solution is 0.1.
[0073] 3) The CIGS absorption layer on the growth substrate is placed in a reaction container containing the mixed solution for heating reaction at a temperature of 80°C for 30 minutes. After the reaction is completed, the temperature is cooled to room temperature, and a CdZn (O, S) buffer layer film is grown on the surface of the CIGS absorption layer. After taking it out, it is rinsed with deionized water and blown dry with nitrogen.
[0074] Example 2
[0075] Similar to Example 1, except that the concentration of cadmium sulfate is 0.45 mmol / L, and the molar ratio of the cadmium source to the zinc source in the mixed solution is 0.01.
[0076] Example 3
[0077] Similar to Example 1, except that the concentration of cadmium sulfate is 0.09 mmol / L, and the molar ratio of the cadmium source to the zinc source in the mixed solution is 0.002.
[0078] Example 4
[0079] Similar to Example 1, except that the concentration of cadmium sulfate is 0.045 mmol / L, and the molar ratio of the cadmium source to the zinc source in the mixed solution is 0.001.
[0080] Comparative Example 1
[0081] 1) The CIGS absorption layer used as the growth substrate is cleaned in an organic solvent and clean water respectively.
[0082] 2) Mix the zinc sulfate solution and the trisodium citrate solution, add 25% ammonia water by mass, increase the amount of ammonia water according to the real-time monitoring value of pH, and then add thiourea solution. The final pH value of the solution is 10.5.
[0083] In the obtained mixed solution, the concentration of zinc sulfate was 0.045 mol / L, the concentration of trisodium citrate was 0.045 mol / L, the concentration of thiourea was 0.15 mol / L, and the pH value of the mixed solution was 10.5.
[0084] 3) The CIGS absorption layer on the growth substrate is placed in a reaction container containing the mixed solution for heating reaction at a temperature of 80°C for 30 minutes. After the reaction is completed, the temperature is cooled to room temperature, and a Zn(O,S) cadmium-free buffer layer film can be grown on the surface of the CIGS absorption layer. After taking it out, rinse it with deionized water and blow dry it with nitrogen.
[0085] Comparative Example 2
[0086] Similar to Example 1, except that: in the mixed solution, the concentration of cadmium sulfate is 0.15 mol / L, the concentration of zinc sulfate is 0.2 mol / L, the concentration of the complexing agent ammonium sulfate is 0.1 mol / L, the concentration of thiourea is 1 mol / L, the concentration of the pH adjusting agent ammonia water is 0.5 mol / L, and the molar ratio of the cadmium source to the zinc source in the mixed solution is 3:4. The reaction temperature is 85° C. and the reaction time is 35 min.
[0087] Comparative Example 3
[0088] Similar to Example 1, except that: in the mixed solution, the concentration of cadmium nitrate is 0.006 mol / L, the concentration of zinc chloride is 0.1 mol / L, no complexing agent is used, and the concentration of thiourea is 0.1 mol / L. The reaction temperature is 65° C. and the reaction time is 70 min.
[0089] Comparative Example 4
[0090] Similar to Example 1, except that the total concentration of cadmium chloride and zinc chloride is 0.1 mol / L, the molar ratio of the cadmium source to the zinc source in the mixed solution is 4:1, triethanolamine is used as a complexing agent, the concentration of thiourea is 0.1 mol / L, the reaction temperature is 70° C., and the reaction time is 60 min.
[0091] Comparative Example 5
[0092] Similar to Comparative Example 4, except that the molar ratio of the cadmium source to the zinc source in the mixed solution is 1:1.
[0093] Comparative Example 6
[0094] Similar to Comparative Example 4, except that the molar ratio of the cadmium source to the zinc source in the mixed solution is 1:4.
[0095] The solar cell buffer layer prepared in Examples 1-4 was observed by scanning electron microscope, and the obtained SEM images are as follows: Figure 1-8 As shown by Figure 1-8 It can be seen that the surface of the solar cell buffer layer prepared by the method of the present invention is smooth and free of cracks, and has no obvious defects such as attachments and pinholes. The film surface quality is high and no further surface treatment is required after the water bath, so it can be directly used in the device structure of the thin-film solar cell.
[0096] The solar cell buffer layers prepared in Examples 1-4 and Comparative Examples 1-6 were subjected to EDS testing to obtain the ratio of Cd / (Zn+Cd) in the solar cell buffer layers, see Table 1.
[0097] The solar cell buffer layers prepared in Examples 1-4 and Comparative Examples 1-6 were subjected to XPS testing to obtain the Cd / (Zn+Cd) ratio in the solar cell buffer layer and the S / (O+S)-film EDS ratio, see Table 1 and Fig.11 .
[0098] The solar cell buffer layers prepared in Examples 1-4 and Comparative Examples 1-6 were tested for light transmittance, and the optical band gap of the CdZn(O,S) film was obtained by linear fitting of the absorption edge in the sample transmission spectrum. The weighted average transmittance and reflectivity of the solar cell buffer layer were obtained as shown in Table 1 and Fig. 9 , Fig.10 .
[0099] The composition and optical properties of the films prepared from the materials of the examples and comparative examples of the present application are shown in Table 1 below:
[0100] Table 1
[0101]
[0102]
[0103] It should be noted that the XPS test can analyze the chemical states of Cd, Zn, O, and S in the CdZn(O,S) film and determine the Cd and S contents in the CdZn(O,S) film. Fig.11The spectrum shown was obtained after Ar sputtering for 60s to remove contaminants and adsorbates on the film surface. Taking the CdZn(O,S) film prepared in Example 2 with a molar ratio of cadmium source to zinc source of 0.01 as an example, the presence of Zn, Cd, O, and S signals in the spectrum indicates that the film has quaternary properties. The center of the Cd3d peak is about 404.47eV, close to CdZnO (404.8eV), indicating that Cd is present in the CdZn(O,S) film. 2+ The Zn2p signal peak is at 1021.15 eV, which is exactly between the corresponding values of ZnO (1020.4 eV) and ZnS (1022.4 eV), confirming that Zn in CdZn(O,S) film 2+ The intermediate chemical state of oxygen sulfide. The center of the O1s peak is located at 530.56eV, which corresponds to the bulk oxygen in the CdZn(O,S) film, which is very consistent with the binding energy of O2 in the CdZnO and ZnOS alloy films. The S2p center is located at 160.83eV, which is basically consistent with the peak position of the CdZn(O,S) quaternary alloy obtained by PLD preparation of sapphire substrates in the literature. The XPS analysis results show that both Cd and S have been completely dissolved and occupied the positions of Zn and O in the ZnO lattice, respectively, thus forming a CdZn(O,S) quaternary alloy. The composition of the CdZn(O,S) film was quantified by using Cd3d, Zn 2p, S 2p and O1s energy level signals, and the results are shown in Table 1. As the cadmium source concentration and its ratio to the zinc source concentration gradually decrease, the Cd content in the film decreases from 94% to 0, while the S content can be reduced from 74% to 36%, which is due to the fact that the cationic Cd 2+ 、Zn 2+ With anion S 2 , O 2- The Cd content in the film is significantly higher than that in the solution, which can be attributed to the different deposition rates. 2+ The reaction rate constant Ksp is greater than that of Zn 2+ Therefore, when the Cd concentration in the solution is only 1% of the Zn concentration, but the Cd content in the film is 0.22, the single-phase CdZn(O,S) film can accommodate up to about 50% S; when the Cd concentration in the solution is only 10% of the Zn concentration, the Cd content in the film is 0.94 and can accommodate up to about 74% S, while the S content limit in Comparative Example 1 is 0.31±0.02. 2+ Zn 2+ and S 2- For O 2- The synergistic effect of co-substitution contributes to the chemically non-equilibrium growth characteristics of quaternary CdZn(O,S) films deposited by chemical water bath deposition.
[0104] The EDS and XPS analysis of the CdZn(O,S) film composition showed that, firstly, the Cd / (Zn+Cd) ratio in the CdZn(O,S) film prepared by the method of the embodiment of the present invention is much larger than the ratio of cadmium in the solution. This is because the reaction rate between Cd cations and anions is greater than the reaction rate between Zn cations and anions. At the same time, the effect of the complexing agent further promotes the reflection of the difference in reaction rates between the two in the film.
[0105] Secondly, the presence of Cd in the CdZn(O,S) film indicates that Cd successfully replaced Zn and entered the film components. When the molar ratio of Cd / (Zn+Cd) in the solution is greater than 0.01, the obtained film maintains a crystal structure dominated by CdS; when the molar ratio of Cd / (Zn+Cd) in the solution is 0.01, CdS and ZnS crystal structures coexist; when the molar ratio of Cd / (Zn+Cd) in the solution is far less than 0.01, it is converted into a crystal structure dominated by ZnS.
[0106] Again, the S / (S+O) in the CdZn(O,S) film is significantly higher than that of the Zn(O,S) film prepared in Comparative Example 1. Therefore, the dual adjustability of the film components Cd / (Zn+Cd) and S / (S+O) and their wide range of variation significantly increase the control range of the CdZn(O,S) film in terms of lattice, band gap, etc., which means that the control of optimizing the matching between the buffer layer and the CIGS absorption layer is broadened.
[0107] In summary, according to the data in Table 1 above, it is found that according to the method of Comparative Example 1, that is, when the reaction solution does not contain a cadmium source, the S / (S+O) ratio of the prepared Zn(O,S) film is 0.31, indicating that the proportion of S oxygen element in the film composition is too low, which makes its matching optimization range as a buffer layer and a CIGS absorption layer narrow.
[0108] According to the method of the embodiment of the present invention, by adding and regulating the precise concentration and ratio of the cadmium source and the zinc source in the reaction solution, the prepared CdZn (O, S) film is of good quality, smooth, crack-free, uniform particle size, and free of obvious defects such as attachments and pinholes. The prepared solar cell buffer layer was subjected to EDS testing, and it was found that the ratio of Cd / (Zn+Cd) in the solar cell buffer layer was 0.03-0.81. The prepared solar cell buffer layer was subjected to XPS testing, and the obtained Cd / (Zn+Cd) ratio in the solar cell buffer layer was 0-0.94, and the S / (O+S) ratio was 0.36-0.74, indicating that the proportion of sulfur in the film composition increased, which enables it to be used as a buffer layer and CIGS absorption layer Matching can be improved, further bringing a positive effect on device efficiency.
[0109] Through the film transmittance test, it was found that the weighted average transmittance of the CdZn(O,S) film obtained by doping was significantly higher than that of the Zn(O,S) film without cadmium (Comparative Example 1) and the CdZn(O,S) prepared by the conventional method in the wavelength range of 350-1300nm, and the transmittance in Comparative Examples 2-3 was significantly reduced. The Hall effect test results showed that the carrier concentration of the prepared CdZn(O,S) film was 10 16 Two orders of magnitude higher than conventional methods.
[0110] Compared with the embodiments of the present invention, in Comparative Example 2, a high-concentration cadmium solution and a high-ratio cadmium solution are used, the Cd / (Zn+Cd) ratio control range is not large, and the transmittance is poor.
[0111] Compared with the embodiments of the present invention, even if the concentration and proportion of the cadmium solution are reduced in Comparative Example 3, the film permeability is not good when no complexing agent is used.
[0112] Compared with the embodiments of the present invention, in Comparative Examples 4-6, even if the cadmium source concentration is adjusted within the range of 0.2-0.8, the adjustable range of S / (O+S) is still narrow.
[0113] In addition, in the process of preparing the solar cell buffer layer, the present invention reduces the amount of raw materials, especially the amount of cadmium solution, thereby reducing the production cost, especially significantly reducing the treatment cost of cadmium-containing waste liquid.
[0114] Obviously, the above embodiments of the present application are merely examples for clearly illustrating the present application, and are not intended to limit the implementation methods of the present application. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all implementation methods here. All obvious changes or modifications derived from the technical solutions of the present application are within the spirit scope covered by the present application.
Claims
1. A solar cell buffer layer, characterized in that: The solar cell buffer layer is a CdZn(O,S) film, wherein the Cd / (Zn+Cd) ratio ranges from 0.03 to 0.94, and the S / (S+O) ratio ranges from 0.36 to 0.
74.
2. The solar cell buffer layer according to claim 1, characterized in that: The Cd / (Zn+Cd) ratio ranges from 0.03 to 0.
81.
3. A method for preparing a solar cell buffer layer, characterized in that: The method comprises: placing the growth substrate in a mixed solution comprising a cadmium source, a zinc source, a complexing agent, a sulfur source and a pH adjuster for contact; Wherein, in the mixed solution, the molar ratio of the cadmium source to the zinc source is (0.001-0.1):1, the concentration of the cadmium source is 0.045mmol / L-4.5mmol / L, and the pH value of the mixed solution is 10.3-11.
4. The method for preparing a solar cell buffer layer according to claim 3, characterized in that: The molar ratio of the cadmium source, the zinc source, the complexing agent and the sulfur source is (0.001-0.1):1:(0.75-1.25):(3-8).
5. The method for preparing a solar cell buffer layer according to claim 1, characterized in that: The contact conditions include: contact temperature of 75-90° C. and contact time of 10-40 min.
6. The method for preparing a solar cell buffer layer according to claim 1, characterized in that: The zinc source is selected from at least one of zinc nitrate, zinc acetate, zinc oxalate, zinc sulfate and zinc chloride.
7. The method for preparing a solar cell buffer layer according to claim 1, characterized in that: The cadmium source is selected from at least one of cadmium nitrate, cadmium acetate, cadmium oxalate, cadmium sulfate and cadmium chloride.
8. The method for preparing a solar cell buffer layer according to claim 1, characterized in that: The complexing agent is selected from at least one of citric acid, sodium citrate, tartaric acid, sodium tartrate, nitrilotriacetic acid, trisodium nitrilotriacetate, and triethanolamine; and / or, The sulfur source is selected from at least one of thiourea, thioacetamide and sodium thiosulfate.
9. The method for preparing a solar cell buffer layer according to claim 1, characterized in that: The pH regulator is selected from at least one of sodium hydroxide, ammonia water, hydrazine and hydrazine.
10. A solar cell buffer layer prepared by the preparation method according to any one of claims 3 to 9.