Preparation method of vanadium electrolyte taking low-purity ammonium vanadate as raw material

By using low-purity ammonium vanadate as raw material and combining oxalic acid dissolution, bipolar membrane electrodialysis, and electrolysis processes, vanadium electrolyte is prepared. This solves the problems of high auxiliary material consumption and high wastewater treatment costs in existing technologies, and achieves low-cost and high-efficiency preparation of vanadium electrolyte, which is suitable for the production of various acidic electrolytes.

CN119009044APending Publication Date: 2024-11-22WONTAI POWER CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411079985.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing vanadium electrolyte preparation processes suffer from problems such as high consumption of auxiliary materials, high wastewater treatment costs, and poor compatibility with chlorine-based electrolytes.

Method used

Using low-purity ammonium vanadate as raw material, vanadium hydroxide and vanadium hydroxide intermediates are prepared through oxalic acid dissolution, bipolar membrane electrodialysis and electrolysis. They are then dissolved in acid solution to obtain a positive electrode (+4 valence), a negative electrode (+3 valence), or a vanadium electrolyte with a valence state between +4 and +3, either sulfate-based or hydrochloric acid-based.

Benefits of technology

It achieves low consumption of auxiliary materials, low wastewater treatment cost, good compatibility with chlorine-based electrolytes, no wastewater generation, high added value of by-product ammonia water, and a wide range of vanadium electrolyte products, suitable for the production of various acidic electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009044A_ABST
    Figure CN119009044A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a vanadium electrolyte by taking low-purity ammonium vanadate as a raw material. The method comprises the following steps: S1, selecting one or two of a step S2-1 and a step S2-2; and S3, dissolving, reducing and removing impurities to obtain a first solution; s2-1, performing bipolar membrane electrodialysis on the first solution obtained in S1 to obtain a first intermediate product; s2-2, performing electrolytic reduction on the first solution obtained in the step S1 to obtain a second solution, and performing bipolar membrane electrodialysis on the second solution to obtain a second intermediate product; and S3, dissolving the first intermediate product obtained in the step S2-1 and / or the second intermediate product obtained in the step S2-2 in an acid solution to obtain the vanadium electrolyte. According to the method, a working section of preparing vanadium pentoxide through roasting is not needed, the process is short, safety is high, the vanadium electrolyte is directly prepared through an electrodialysis method, new impurities are not introduced in the reaction process, the value of by-product ammonia water is high, the production cost of the electrolyte can be effectively reduced, and the production requirements of various acid series electrolytes are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of vanadium electrolyte, and in particular relates to a method for preparing a vanadium electrolyte using low-purity ammonium vanadate as a raw material. Background Art

[0002] All-vanadium liquid flow battery (abbreviated as vanadium battery) is a new type of liquid flow battery with the advantages of high safety, high stability, long life, green environmental protection, and independent adjustable capacity and power. It is widely used in large-scale energy storage systems. Vanadium electrolyte is the key material of all-vanadium liquid flow battery system and the energy carrier for the mutual conversion of chemical energy and electrical energy. Its purity directly affects the performance and service life of vanadium battery.

[0003] Ammonium vanadate includes ammonium metavanadate (NH4VO3, referred to as AMV) and ammonium polyvanadate (NH4V3O8, referred to as APV). Currently, low-purity ammonium vanadate is the main vanadium raw material for preparing vanadium electrolyte. The existing preparation technology is mainly divided into the following two types according to the length of the production process:

[0004] 1) Long process method: low-purity ammonium vanadate is used as the raw material, and high-purity ammonium vanadate is obtained through alkali dissolution, impurity removal, and vanadium precipitation, and then high-purity vanadium pentoxide or low-valent vanadium oxide (vanadium trioxide, vanadium dioxide or a mixture of the two) is obtained through calcination or reduction calcination. High-purity vanadium pentoxide is reduced by electrolysis or chemical reduction combined with electrolysis to obtain a 3.5-valent electrolyte; low-valent vanadium oxide is directly dissolved in acid according to the composition ratio to obtain a 3.5-valent vanadium electrolyte. This method consumes a large amount of auxiliary materials such as caustic soda flakes and ammonium salts, and the cost of treating vanadium precipitation wastewater is high; the calcination process requires the use of high-temperature equipment such as rotary kilns, which occupy a large area and have high energy consumption. Reduction calcination requires the use of flammable and explosive raw materials such as liquid ammonia and hydrogen, and the production safety is low.

[0005] 2) Short process method: low-purity ammonium vanadate is subjected to steps such as dissolution reduction and pH adjustment to obtain low-purity tetravalent vanadium oxysulfate solution, and then subjected to steps such as extraction and stripping to obtain high-purity tetravalent vanadium electrolyte, which is further electrolytically reduced to obtain 3.5-valent vanadium electrolyte. This method does not require the step of calcination to obtain vanadium oxide, which simplifies the production process and improves production safety. However, since the process produces a raffinate containing a large amount of sulfuric acid and impurities, the wastewater treatment process also requires the consumption of a large amount of caustic soda, and the wastewater treatment cost is high; the extractant is easy to remain in the electrolyte product, and further deep degreasing is required before it can be used; this method cannot be separated from the electrolytic reduction technology in the process of adjusting the valence state of the vanadium element, and the existing electrolytic reduction technology generally uses a titanium plate with an oxygen-evolving precious metal coating as the anode, which is not suitable for the preparation of chlorine-containing hydrochloric acid or mixed acid-based electrolytes.

[0006] In summary, the existing vanadium electrolyte preparation process has problems such as large consumption of auxiliary materials, high wastewater treatment cost and poor compatibility with chlorine-based electrolytes. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a method for preparing a vanadium electrolyte using low-purity ammonium vanadate as a raw material. The present invention first dissolves and reduces low-purity ammonium vanadate in an oxalic acid solution, obtains an impurity-free oxalate solution after filtration, and then passes it into a bipolar membrane electrodialysis device to obtain vanadium hydroxide (VO(OH)2), and / or passes it into an electrolysis device to obtain an oxalate solution with a vanadium valence of about +3, further passes the oxalate solution with a vanadium valence of about +3 through bipolar membrane electrodialysis to obtain vanadium hydroxide (V(OH)3) precipitation and possible vanadium hydroxide, and dissolves the vanadium hydroxide, vanadium hydroxide or a mixture of the two in a sulfuric acid solution, a hydrochloric acid solution or a mixed solution of the two, so as to obtain a positive electrode (+4 valence), a negative electrode (+3 valence) or a sulfate-based or hydrochloric acid-based or mixed acid vanadium electrolyte product with a valence between +4 and +3 (for example, +3.5 valence). The method of the invention has the advantages of low auxiliary material consumption, low wastewater treatment cost, good compatibility with chlorine-based electrolyte, no wastewater generation in the process, and high added value of by-product ammonia water.

[0008] Specifically, the present invention provides a method for preparing a vanadium electrolyte, the method comprising the following steps S1, one or two steps selected from step S2-1 and step S2-2, and step S3:

[0009] S1: low-purity ammonium vanadate, oxalic acid and water are mixed evenly, reacted, and filtered after the reaction is completed to obtain a first solution; wherein the low-purity ammonium vanadate is low-purity ammonium metavanadate or low-purity ammonium polyvanadate, the calcined purity of the low-purity ammonium vanadate is ≤99.5%, and all vanadium elements in the first solution are in the form of VO 2+ exists in the form of;

[0010] S2-1: sending part or all of the first solution obtained in step S1 to the salt chamber of a first bipolar membrane electrodialysis device for electrodialysis, filtering and drying the product in the alkali chamber of the first bipolar membrane electrodialysis device to obtain a first intermediate product, wherein the first intermediate product is VO(OH)2;

[0011] S2-2: sending part or all of the first solution obtained in step S1 to the cathode cell of an electrolysis device for electrolysis to obtain a second solution, wherein the average valence of the vanadium element in the second solution is +3.00 to +3.03, sending the second solution to the salt chamber of a second bipolar membrane electrodialysis device for electrodialysis, filtering and drying the product in the alkali chamber of the second bipolar membrane electrodialysis device to obtain a second intermediate product, wherein the second intermediate product is V(OH)3 and possibly VO(OH)2;

[0012] S3: Dissolve the first intermediate product obtained in step S2-1 alone in an acid solution, or dissolve the second intermediate product obtained in step S2-2 alone in an acid solution, or dissolve the first intermediate product obtained in step S2-1 and the second intermediate product obtained in step S2-2 together in an acid solution to obtain a vanadium electrolyte in which the average valence of the vanadium element is +4, +3, or between +4 and +3.

[0013] In one or more embodiments, in step S1, when the low-purity ammonium vanadate is low-purity ammonium metavanadate, the low-purity ammonium metavanadate and oxalic acid are added in a molar ratio of vanadium element to oxalic acid of 1:(2.2-2.5).

[0014] In one or more embodiments, in step S1, when the low-purity ammonium vanadate is low-purity ammonium polyvanadate, the low-purity ammonium polyvanadate and oxalic acid are added in a molar ratio of vanadium element to oxalic acid of 3:(5.5-6.0).

[0015] In one or more embodiments, the concentration of vanadium in the reaction system in step S1 is 0.5 mol / L to 1.0 mol / L.

[0016] In one or more embodiments, the reaction in step S1 is carried out under stirring at a reaction temperature of 50°C to 60°C.

[0017] In one or more embodiments, when the low-purity ammonium vanadate used in step S1 is low-purity ammonium metavanadate, the electrodialysis time in step S2-1 is controlled as follows: T1 = 5·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C V is the vanadium element concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device.

[0018] In one or more embodiments, when the low-purity ammonium vanadate used in step S1 is low-purity ammonium polyvanadate, the electrodialysis time in step S2-1 is controlled as follows: T1 = 13 / 3·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C Vis the vanadium element concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device.

[0019] In one or more embodiments, the electrolysis time of the electrolysis device in step S2-2 is controlled as follows: T2 = C V ·V2·F / (I2·n2·η2), where T2 is the electrolysis time of the electrolysis device, in seconds; C V is the vanadium concentration of the first solution entering the electrolysis device, in mol / L; V2 is the volume of the first solution entering the electrolysis device, in L; F is the Faraday constant, which is 96485C / mol; I2 is the electrolysis current of the electrolysis device, in A; n2 is the number of electrolysis units of the electrolysis device; η2 is the current efficiency of the electrolysis device.

[0020] In one or more embodiments, when the low-purity ammonium vanadate used in step S1 is low-purity ammonium metavanadate, the electrodialysis time in step S2-2 is controlled as follows: T3 = (1 + N)·C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C V is the vanadium element concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device.

[0021] In one or more embodiments, when the low-purity ammonium vanadate used in step S1 is low-purity ammonium polyvanadate, the electrodialysis time in step S2-2 is controlled as follows: T3 = (1 / 3 + N)·C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C Vis the vanadium element concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device.

[0022] In one or more embodiments, the first bipolar membrane electrodialysis device and the second bipolar membrane electrodialysis device each independently comprise an electrolysis unit or a plurality of electrolysis units connected in series, each electrolysis unit comprising a bipolar membrane, an acid chamber, an anion membrane, a salt chamber, an cation membrane, an alkali chamber and a bipolar membrane, the acid chamber being located between the bipolar membrane and the anion membrane, the salt chamber being located between the anion membrane and the cation membrane, and the alkali chamber being located between the cation membrane and the bipolar membrane; the electrodialysis process adopts a DC power supply, and the current density is 30 mA / cm 2 ~50mA / cm 2 .

[0023] In one or more embodiments, the electrolysis device comprises one or more electrolysis units, each of which comprises a cathode plate, a cathode electrode, a cathode cell, a diaphragm, an anode cell and an anode plate, wherein the cathode plate is made of graphite, the cathode electrode is made of carbon felt or graphite felt, the anode plate is made of titanium, the anode electrolyte is a sulfuric acid solution, and the current density of the electrolysis process is 80 mA / cm 2 ~120mA / cm 2 .

[0024] In one or more embodiments, the method further includes: in step S2-1, the product in the acid chamber of the first bipolar membrane electrodialysis device is recycled to step S1, the product in the salt chamber of the first bipolar membrane electrodialysis device is concentrated by a reverse osmosis system and then recycled as a raw material for the salt chamber of the first bipolar membrane electrodialysis device, and the water produced by the reverse osmosis system is recycled as an ion receiving liquid to the alkali chamber and / or acid chamber of the first bipolar membrane electrodialysis device.

[0025] In one or more embodiments, the method further includes: in step S2-2, the product in the acid chamber of the second bipolar membrane electrodialysis device is reused in step S1, the product in the salt chamber of the second bipolar membrane electrodialysis device is concentrated by a reverse osmosis system and then reused as a raw material for the salt chamber of the second bipolar membrane electrodialysis device, and the water produced by the reverse osmosis system is reused as an ion receiving liquid to the salt chamber and / or acid chamber of the second bipolar membrane electrodialysis device.

[0026] In one or more embodiments, the acid solution in step S3 is a sulfuric acid solution, a hydrochloric acid solution, or a mixture of the two.

[0027] In one or more embodiments, when the acid solution in step S3 is a sulfuric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 2.0 mol / L, and the concentration of sulfate ions is 3 mol / L to 5.5 mol / L.

[0028] In one or more embodiments, when the acid solution in step S3 is a hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 4.0 mol / L, and the concentration of chloride ions is 6 mol / L to 8 mol / L.

[0029] In one or more embodiments, when the acid solution in step S3 is a mixture of a sulfuric acid solution and a hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 3.5 mol / L, the concentration of sulfate ions is 1 mol / L to 3.0 mol / L, and the concentration of chloride ions is 3 mol / L to 6 mol / L. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a schematic flow diagram of a method for preparing a vanadium electrolyte according to some embodiments of the present invention.

[0031] Figure 2 The electrochemical cycle performance test results of the all-vanadium liquid flow battery using the vanadium electrolyte of Example 1 are shown.

[0032] Figure 3 The electrochemical cycle performance test results of the all-vanadium liquid flow battery using the vanadium electrolyte of Example 2 are shown.

[0033] Figure 4 The electrochemical cycle performance test results of the all-vanadium liquid flow battery using the vanadium electrolyte of Example 3 are shown. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the present invention. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this specification shall prevail.

[0035] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0036] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0037] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values ​​within the range (including integers and fractions).

[0038] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0039] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope defined by the present invention.

[0040] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0041] like Figure 1 As shown, the method for preparing a vanadium electrolyte of the present invention comprises the following steps S1, one or two steps selected from step S2-1 and step S2-2, and step S3:

[0042] S1: low-purity ammonium vanadate, oxalic acid and water are mixed evenly, reacted, and filtered after the reaction is completed to obtain a first solution; wherein the low-purity ammonium vanadate is low-purity ammonium metavanadate or low-purity ammonium polyvanadate, and all vanadium elements in the first solution are in the form of VO 2+ exists in the form of;

[0043] S2-1: sending part or all of the first solution obtained in step S1 to the salt chamber of the first bipolar membrane electrodialysis device (bipolar membrane electrodialysis 1#) for electrodialysis, filtering and drying the product in the alkali chamber of the first bipolar membrane electrodialysis device to obtain a first intermediate product, wherein the first intermediate product is VO(OH)2;

[0044] S2-2: sending part or all of the first solution obtained in step S1 to the cathode cell of the electrolysis device for electrolytic reduction to obtain a second solution (trivalent vanadium oxalate solution), wherein the average valence of the vanadium element in the second solution is +3.00 to +3.03, sending the second solution to the salt chamber of the second bipolar membrane electrodialysis device (bipolar membrane electrodialysis 2#) for electrodialysis, filtering and drying the product in the alkali chamber of the second bipolar membrane electrodialysis device to obtain a second intermediate product, wherein the second intermediate product is V(OH)3 and possible VO(OH)2;

[0045] S3: Dissolve the first intermediate product obtained in step S2-1 alone in an acid solution, or dissolve the second intermediate product obtained in step S2-2 alone in an acid solution, or dissolve the first intermediate product obtained in step S2-1 and the second intermediate product obtained in step S2-2 together in an acid solution to obtain a vanadium electrolyte in which the average valence of the vanadium element is +4, +3, or between +4 and +3.

[0046] In the present invention, low-purity ammonium vanadate refers to ammonium vanadate containing impurities. The calcined purity of low-purity ammonium vanadate can be ≤99.5%. In some embodiments, the calcined purity of low-purity ammonium vanadate is 90.0%-99.5%, such as 95.0%-99.5%, 96.0%-95.5%, 97.0%-95.5%.

[0047] In step S1, oxalic acid can be added to the reaction system in the form of anhydrous oxalic acid or hydrated oxalic acid (eg, dihydrate oxalic acid).

[0048] In the present invention, the reaction between low-purity ammonium vanadate and oxalic acid in step S1 is as follows:

[0049] 2NH4VO3+4H2C2O4=2VOC2O4+(NH4)2C2O4+2CO2↑+4H2O

[0050] 2NH4V3O8+10H2C2O4=6VOC2O4+(NH4)2C2O4+6CO2↑+10H2O

[0051] M n+ +C2O4 2- →M(C2O4) n / 2 ↓

[0052] The metal element M in the formula can be one or more of Ca, Cu, Ba, Ag, Fe, Ni, Zn, Mn, Al, Cr, Pb, and Co.

[0053] In the present invention, in order to make the reaction in step S1 more complete, step S1 is carried out under heating conditions, and the heating temperature is preferably 50°C to 60°C, for example, 50°C, 55°C, or 60°C.

[0054] In the present invention, in order to make the reaction in step S1 more complete, the reaction time can be 40 min to 60 min, for example, 40 min, 50 min, or 60 min.

[0055] In the present invention, when the ammonium vanadate is ammonium metavanadate, the ammonium metavanadate and oxalic acid are preferably fed in a ratio of vanadium to oxalic acid of 1:(2.2-2.5), for example, 1:2.3 or 1:2.4. This is conducive to completely converting the vanadium element in the ammonium metavanadate into VO 2+ .

[0056] In the present invention, when the ammonium vanadate is ammonium polyvanadate, the ammonium polyvanadate and oxalic acid are preferably fed in a ratio of vanadium to oxalic acid of 3:(5.5-6.0), such as 3:5.6, 3:5.7, 3:5.8, 3:5.9. This is conducive to completely converting the vanadium element in the ammonium polyvanadate into VO 2+ .

[0057] In the present invention, preferably, the concentration of vanadium element in the reaction system in step S1 is 0.5 mol / L to 1.0 mol / L, for example, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L.

[0058] In the present invention, the following reaction occurs during the electrodialysis process of step S2-1:

[0059] Base chamber: VO 2+ +2OH - =VO(OH)2↓

[0060] Bipolar membrane: H2O→H + +OH -

[0061] Acid room: 2H + +C2O4 2- =H2C2O4

[0062] It should be understood that the vanadium element in the electrodialysis process of step S2-1 comes from the first solution obtained in step S1. The first solution is sent to the salt chamber of the first bipolar membrane electrodialysis device for electrodialysis, and the product in the alkali chamber of the first bipolar membrane electrodialysis device is filtered and dried to obtain ammonia water and the first intermediate product vanadium hydroxide precipitate. In step S2-1, the product in the acid chamber of the first bipolar membrane electrodialysis device can be reused in step S1, the product in the salt chamber of the first bipolar membrane electrodialysis device can be concentrated by a reverse osmosis system and then reused as a raw material for the salt chamber of the first bipolar membrane electrodialysis device, and the water produced by the reverse osmosis system can be reused as an ion receiving liquid in the alkali chamber and / or acid chamber of the first bipolar membrane electrodialysis device.

[0063] In the present invention, preferably, the electrolysis method in the electrodialysis process in step S2-1 is constant current electrolysis.

[0064] In the present invention, the electrodialysis time and electrolysis current of step S2-1 are controlled so that the vanadium element in the alkali chamber is converted into VO(OH)2 as much as possible. To achieve this, when the raw material is ammonium metavanadate, the electrodialysis time of step S2-1 electrodialysis is preferably set to: T1 = 5·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C V is the vanadium concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device. When the raw material is ammonium polyvanadate, the electrodialysis time of step S2-1 electrodialysis is preferably set to: T1 = 13 / 3·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C V is the vanadium element concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device.

[0065] In the present invention, preferably, the electrolysis current value during the electrodialysis process in step S2-1 is 6A to 10A, for example, 6A, 8A, or 10A.

[0066] In the present invention, preferably, the electrolysis time in the electrodialysis process in step S2-1 is 1.3h to 1.8h, for example, it can be 1.3h, 1.34h, 1.4h, 1.5h, 1.51h, 1.6h, or 1.61h.

[0067] In the present invention, the following reaction occurs during the electrolysis process of step S2-2:

[0068] Cathode reaction: VO 2+ +2H + +e - →V 3+ +H2O

[0069] Anode reaction: 2H2O-4e -→4H + +O2↑

[0070] It should be understood that the vanadium element in the electrolysis process of step S2-2 comes from the first solution obtained in step S1. The first solution is sent to the electrolytic reduction device in step S2-2 so that the vanadium element is electrolytically reduced at the cathode to an average valence state of the vanadium element of +3.00 to +3.03, thereby obtaining a second solution.

[0071] In the present invention, preferably, the electrolysis method in the electrolysis device in step S2-2 is constant current electrolysis.

[0072] In the present invention, the electrolysis time and electrolysis current of step S2-2 are controlled so that the vanadium element in the electrolysis device is reduced to an average valence state of +3.00 to +3.03 as much as possible. To achieve this, the electrolysis time of the electrolysis device in step S2-2 is preferably set to: T2 = C V ·V2·F / (I2·n2·η2), where T2 is the electrolysis time of the electrolysis device, in seconds; C V is the vanadium concentration of the first solution entering the electrolysis device, in mol / L; V2 is the volume of the first solution entering the electrolysis device, in L; F is the Faraday constant, which is 96485C / mol; I2 is the electrolysis current of the electrolysis device, in A; n2 is the number of electrolysis units of the electrolysis device; η2 is the current efficiency of the electrolysis device.

[0073] In the present invention, preferably, the electrolysis current value during the electrolysis process in step S2-2 is 3A to 6A, for example, it can be 3A, 3.84A, 4A, 4.80A, 5A, 5.76A, or 6A.

[0074] In the present invention, preferably, the electrolysis time in the electrolysis process in step S2-2 is 1.2h to 1.8h, for example, it can be 1.20h, 1.23h, 1.30h, 1.40h, 1.48h, 1.50h, 1.51h, 1.60h, 1.61h, 1.64h, 1.70h, or 1.80h.

[0075] In the present invention, the following reaction occurs during the electrodialysis process of step S2-2:

[0076] Base chamber: VO 2+ +2OH - =VO(OH)2↓, V 3+ +3OH - =V(OH)3↓

[0077] Bipolar membrane: H2O→H + +OH -

[0078] Acid room: 2H+ +C2O4 2- =H2C2O4

[0079] It should be understood that the vanadium element in the electrodialysis process of step S2-2 comes from the second solution obtained in the electrolysis step of S2-2. The obtained second solution is sent to the salt chamber of the second bipolar membrane electrodialysis device for electrodialysis, and the product of the alkali chamber of the second bipolar membrane electrodialysis device is filtered and vacuum dried to obtain the second intermediate product vanadium hydroxide precipitate and the possible vanadium hydroxide precipitate. In step S2-2, the product in the acid chamber of the second bipolar membrane electrodialysis device can be reused in step S1, the product in the salt chamber of the second bipolar membrane electrodialysis device can be concentrated by the reverse osmosis system and then reused as the raw material of the salt chamber of the second bipolar membrane electrodialysis device, and the water produced by the reverse osmosis system can be reused as an ion receiving liquid in the alkali chamber and / or acid chamber of the second bipolar membrane electrodialysis device.

[0080] In the present invention, preferably, the electrolysis method in the electrodialysis process in step S2-2 is constant current electrolysis.

[0081] In the present invention, the electrodialysis time and electrolysis current of step S2-2 are controlled so that the vanadium element in the alkali chamber is converted into vanadium hydroxide and possible vanadium oxyhydroxide as much as possible. To achieve this, when the raw material is ammonium metavanadate, the electrodialysis time of step S2-2 electrodialysis is preferably set to: T3 = (1 + N)·C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C V is the vanadium concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device. When the raw material is ammonium polyvanadate, the electrodialysis time of step S2-2 electrodialysis is preferably set to: T3 = (1 / 3 + N) · C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C Vis the vanadium element concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device.

[0082] In the present invention, preferably, the electrolysis current value during the electrodialysis process in step S2-2 is 6A to 10A, for example, 6A, 8A, or 10A.

[0083] In the present invention, preferably, the electrolysis time in the electrodialysis process in step S2-2 is 1.0 h to 1.3 h, for example, it can be 1.0 h, 1.08 h, 1.10 h, 1.20 h, 1.29 h, or 1.30 h.

[0084] In the present invention, in step S3, the vanadium oxyhydroxide and vanadium hydroxide obtained in step S2-1 and step S2-2 are dissolved in an acid solution separately or in a certain molar ratio (e.g., 1:1) to obtain a vanadium electrolyte. Preferably, the acid solution is sulfuric acid or hydrochloric acid or a mixture of the two.

[0085] More preferably, when the acid solution in step S3 is a sulfuric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5mol / L to 2.0mol / L, for example, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L, 2.0mol / L; the concentration of sulfate ion is 3mol / L to 5.5mol / L, for example, 3.0mol / L, 3.5mol / L, 4.0mol / L, 4.5mol / L, 5.0mol / L, 5.5mol / L;

[0086] When the acid solution in step S3 is a hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5mol / L to 4.0mol / L, for example, 1.5mol / L, 2.0mol / L, 3.0mol / L, 4.0mol / L; the concentration of chloride ion is 6mol / L to 8mol / L, for example, 6.0mol / L, 7.0mol / L, 8.0mol / L;

[0087] When the acid solution in step S3 is a mixture of sulfuric acid solution and hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5mol / L to 3.5mol / L, for example, it can be 1.5mol / L, 2.0mol / L, 3.0mol / L, 3.5mol / L; the concentration of sulfate ions is 1.0mol / L to 3.0mol / L, for example, it can be 1.0mol / L, 2.0mol / L, 3.0mol / L; the concentration of chloride ions is 3mol / L to 6mol / L, for example, it can be 3.0mol / L, 4.0mol / L, 5.0mol / L, 6.0mol / L.

[0088] In a preferred embodiment, the first bipolar membrane electrodialysis device and the second bipolar membrane electrodialysis device each independently comprise an electrolysis unit or a plurality of electrolysis units connected in series, each electrolysis unit comprises a bipolar membrane, an acid chamber, an anion membrane, a salt chamber, an cation membrane, an alkali chamber and a bipolar membrane, the acid chamber is located between the bipolar membrane and the anion membrane, the salt chamber is located between the anion membrane and the cation membrane, and the alkali chamber is located between the cation membrane and the bipolar membrane; the electrodialysis process preferably uses a DC power supply; the current density of the electrodialysis process is preferably 30 mA / cm 2 ~50mA / cm 2 , for example 35mA / cm 2 , 40mA / cm 2 , 45mA / cm 2 .

[0089] In a preferred embodiment, the electrolysis device comprises one or more electrolysis units, each of which comprises a cathode plate, a cathode electrode, a cathode cell, a diaphragm, an anode cell and an anode plate. The cathode plate is preferably made of graphite, the cathode electrode is preferably made of carbon felt or graphite felt, the anode plate is preferably made of titanium, and the anode electrolyte is preferably a sulfuric acid solution. The current density of the electrolysis process is preferably 80 mA / cm 2 ~120mA / cm 2 , for example 90mA / cm 2 , 100mA / cm 2 , 110mA / cm 2 .

[0090] Compared with the prior art, the present invention has the following beneficial effects:

[0091] 1) Low amount of auxiliary materials: The present invention uses low-purity ammonium vanadate as a raw material, and prepares the electrolyte through a bipolar membrane electrodialysis process, making full use of the reducing property, acidity and impurity removal effect of oxalic acid, without the need for additional impurity remover, caustic soda flakes and vanadium precipitation agent consumption;

[0092] 2) Short process and high safety: The present invention adopts bipolar membrane electrodialysis process to replace vanadium precipitation-calcination or extraction to achieve the purpose of vanadium ammonium separation, without going through the vanadium oxide preparation step, without high-temperature calcination equipment, short process and improved process safety;

[0093] 3) The present invention uses a bipolar membrane electrodialysis process, which makes the process resource utilization high, no wastewater discharge, sufficient recycling of oxalic acid, and high economic value of by-product ammonia water;

[0094] 4) Wide range of products: In the present invention, vanadium hydroxide is easily soluble in various acidic solutions, and the reaction conditions are low, which can meet the production needs of various acidic electrolytes. The vanadium ion concentration can be adjusted in a wide range; +3-valent, +4-valent and +3.5-valent electrolytes can be produced.

[0095] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased from commercial sources. In the present invention, concentrated sulfuric acid refers to a sulfuric acid solution having a sulfuric acid concentration of 98wt%.

[0096] In the present invention, the calcined purity = the mass of vanadium pentoxide in the product obtained after calcination, deammoniation and dehydration of low-purity ammonium vanadate / the total mass of the product*100%.

[0097] In the present invention, the burning rate = the mass of the product obtained after calcination, deamination and dehydration of low-purity ammonium vanadate / the mass before calcination*100%.

[0098] The first bipolar membrane electrodialysis device used in Examples 1-3 comprises 10 electrolysis units connected in series, each of which comprises a bipolar membrane, an acid chamber, an anion membrane, a salt chamber, a cation membrane, an alkali chamber and a bipolar membrane, wherein the acid chamber is located between the bipolar membrane and the anion membrane, the salt chamber is located between the anion membrane and the cation membrane, and the alkali chamber is located between the cation membrane and the bipolar membrane; a direct current power supply is used in the electrodialysis process; the effective area of ​​the diaphragm (bipolar membrane, anion membrane and cation membrane) is 200 cm 2 ; The current efficiency is 82.5%.

[0099] The second bipolar membrane electrodialysis device used in Examples 1-3 comprises 10 electrolysis units connected in series, each of which comprises a bipolar membrane, an acid chamber, an anion membrane, a salt chamber, a cation membrane, an alkali chamber and a bipolar membrane, wherein the acid chamber is located between the bipolar membrane and the anion membrane, the salt chamber is located between the anion membrane and the cation membrane, and the alkali chamber is located between the cation membrane and the bipolar membrane; a direct current power supply is used in the electrodialysis process; the effective area of ​​the diaphragm (bipolar membrane, anion membrane and cation membrane) is 200 cm 2 ; The current efficiency is 82.5%.

[0100] The electrolysis device used in Examples 1-3 comprises three electrolysis units, each of which comprises a cathode plate, a cathode electrode, a cathode pool, a diaphragm, an anode pool and an anode plate. The cathode plate is made of graphite, the cathode electrode is made of carbon felt or graphite felt, the anode plate is made of titanium, and the anode electrolyte is a sulfuric acid solution; the effective area of ​​the diaphragm is 48 cm 2 ; The current efficiency is 93.5%.

[0101] Example 1

[0102] This embodiment adopts the method of the present invention to prepare a vanadium electrolyte by the following steps:

[0103] S1: Weigh 125.7 g of low-purity ammonium metavanadate (burning rate 74.1%, burning purity 97.7%) obtained by extracting vanadium from stone coal in a factory in Gansu and 277.2 g of dihydrated oxalic acid, add them to 2 L of water, heat to 50 ° C under stirring conditions and keep the temperature for 60 minutes. After the reaction is completed, filter and remove impurities to obtain a first solution containing vanadium oxalate and ammonium oxalate. All vanadium in the first solution is converted into VO 2+ The vanadium concentration of the first solution is 0.496 mol / L;

[0104] S2-1: Send 1L of the first solution obtained in S1 to the salt chamber of the first bipolar membrane electrodialysis device for electrodialysis, set the current value to 6A, and perform electrodialysis for 1.34h (the electrodialysis time T1 satisfies the above formula T1=5·C V ·V1·F / (I1·n1·η1)), the base chamber product was filtered to obtain vanadyl hydroxide (VO(OH)2) precipitate, which weighed 49.65g after drying, and the comprehensive yield of vanadyl hydroxide was 98.31%;

[0105] S2-2: Send 1L of the first solution obtained in S1 to the cathode cell of the electrolysis device, set the current value to 3.84A, and electrolyze for 1.23h (the electrolysis time T2 satisfies the above formula T2=C V ·V2·F / (I2·n2·η2)), the vanadium concentration in the solution was measured to be 0.495 mol / L, and the average valence of vanadium was +3.01. The solution was sent to the salt chamber of the second bipolar membrane electrodialysis device for electrodialysis. The current value was set to 6A and the electrolysis was performed for 1.08h (the electrodialysis time T3 satisfied the above formula T3=(1+N)·C V ·V3·F / (I3·n3·η3)), the alkali chamber product was filtered to obtain vanadium hydroxide (V(OH)3) precipitate and a very small amount of vanadyl hydroxide (VO(OH)2) precipitate, which weighed 50.49g after vacuum drying (all products were regarded as vanadium hydroxide), and the comprehensive yield of vanadium hydroxide was 97.72%;

[0106] S3: Add 116.8 mL of concentrated sulfuric acid to 0.35 L of water to obtain a dilute sulfuric acid solution, take 42.93 g of vanadium hydroxide (VO(OH)2) obtained in S2-1 and 43.35 g of vanadium hydroxide (V(OH)3) obtained in S2-2 and add them to the dilute sulfuric acid solution, stir and react for 20 minutes, then add water to make the volume to 0.5 L to obtain a sulfate-based vanadium electrolyte product with a vanadium element concentration of 1.70 mol / L, a sulfate ion concentration of 4.30 mol / L, and an average valence of the vanadium element of +3.5.

[0107] Test the performance of vanadium electrolyte: Assemble a single test vanadium battery using graphite electrode, flexible graphite plate and Nafion membrane as materials, and inject 100mL of the above product electrolyte into the effective area of ​​48cm 2 In the positive and negative electrodes of the vanadium battery, at 150mA / cm 2 The constant current charge and discharge test was conducted for 50 cycles at a current density of 1.55V for charging and 1V for discharging. The test results are as follows: Figure 2 As shown, the battery operates normally with an energy efficiency of 82.55% on average.

[0108] Example 2

[0109] This embodiment adopts the method of the present invention to prepare a vanadium electrolyte by the following steps:

[0110] S1: Weigh 151.8 g of low-purity ammonium polyvanadate (burning rate 91.7%, burnt purity 98.0%) obtained by extracting vanadium from vanadium slag of a factory in Heilongjiang and 378.0 g of dihydrated oxalic acid, add them to 2 L of water, heat to 55 ° C under stirring conditions and keep the temperature for 50 minutes. After the reaction is completed, filter and remove impurities to obtain a first solution containing vanadium oxalate and ammonium oxalate. All vanadium in the first solution is converted into VO 2+ The solution vanadium concentration was measured to be 0.745 mol / L.

[0111] S2-1: Send 1L of the first solution obtained in S1 to the salt chamber of the first bipolar membrane electrodialysis device for electrodialysis, set the current value to 8A, and electrolyze for 1.51h (the electrodialysis time T1 satisfies the above formula T1=13 / 3·C V ·V1·F / (I1·n1·η1)), the base chamber product was filtered to obtain vanadyl hydroxide (VO(OH)2) precipitate, which weighed 74.468g after drying, and the comprehensive yield of vanadyl hydroxide was 98.31%;

[0112] S2-2: Send 1L of the first solution obtained in S1 to the cathode cell of the electrolysis device, set the current value to 4.80A, and electrolyze for 1.48h (the electrolysis time T2 satisfies the above formula T2=C V·V2·F / (I2·n2·η2)), the solution vanadium ion concentration was measured to be 0.736mol / L, and the average valence of vanadium element was +3.02. The solution was sent to the salt chamber of the second bipolar membrane electrodialysis device for electrodialysis. The current value was set to 8A and the electrolysis was performed for 1.20h (the electrodialysis time T3 satisfied the above formula T3=(1 / 3+N)·C V ·V3·F / (I3·n3·η3)), the alkali chamber product was filtered to obtain vanadium hydroxide (V(OH)3) precipitate and a very small amount of vanadyl hydroxide (VO(OH)2) precipitate, which weighed 75.072g after vacuum drying (all products were regarded as vanadium hydroxide), and the comprehensive yield of vanadium hydroxide was 97.06%;

[0113] S3: Add 54.3 mL of concentrated sulfuric acid and 166.7 mL of concentrated hydrochloric acid to 0.25 L of water to obtain a mixed acid solution, then take 42.93 g of vanadium hydroxide (VO(OH)2) obtained in S2-1 and 43.35 g of vanadium hydroxide (V(OH)3) obtained in S2-2 and add them to the mixed acid solution, stir the reaction for 30 minutes, and then add water to make the volume to 0.5 L to obtain a mixed acid vanadium electrolyte product with a vanadium element concentration of 2.0 mol / L, a sulfate ion concentration of 2.0 mol / L, a chloride ion concentration of 2.0 mol / L, and an average valence state of the vanadium element of +3.5.

[0114] Test the performance of vanadium electrolyte: Assemble a single test vanadium battery using graphite electrode, flexible graphite plate and Nafion membrane as materials, and inject 100mL of the above product electrolyte into the effective area of ​​48cm 2 In the positive and negative electrodes of the vanadium battery, at 150mA / cm 2 The constant current charge and discharge test was conducted for 50 cycles at a current density of 1.55V for charging and 1V for discharging. The test results are as follows: Figure 3 As shown, the battery operates normally with an energy efficiency of 82.64% on average.

[0115] Example 3

[0116] This embodiment adopts the method of the present invention to prepare a vanadium electrolyte by the following steps:

[0117] S1: Weigh 234.17 g of low-purity ammonium polyvanadate (burning rate 78.4%, burnt purity 99.1%) obtained by extracting vanadium from vanadium slag of a factory in Xinjiang and 504.0 g of dihydrated oxalic acid into 2 L of water, heat to 60°C under stirring and keep the temperature for 40 min. After the reaction is completed, filter and remove impurities to obtain a first solution containing vanadium oxalate and ammonium oxalate. All vanadium in the first solution is converted into VO 2+ The solution vanadium concentration was measured to be 0.990 mol / L.

[0118] S2-1: Send 1L of the first solution obtained in S1 to the salt chamber of the first bipolar membrane electrodialysis device for electrodialysis, set the current value to 10A, and electrolyze for 1.61h (the electrodialysis time T1 satisfies the above formula T1=13 / 3·C V ·V1·F / (I1·n1·η1)), the base chamber product was filtered to obtain vanadyl hydroxide (VO(OH)2) precipitate, which weighed 98.990g after drying, and the comprehensive yield of vanadyl hydroxide was 98.01%;

[0119] S2-2: Send 1L of the first solution obtained in S1 to the cathode cell of the electrolysis device, set the current value to 5.76A, and electrolyze for 1.64h (the electrolysis time T2 satisfies the above formula T2=C V ·V2·F / (I2·n2·η2)), the solution vanadium ion concentration was measured to be 0.988mol / L, and the average valence of vanadium element was +3.01. The solution was sent to the salt chamber of the second bipolar membrane electrodialysis device for electrodialysis. The current value was set to 10A and the electrolysis was performed for 1.29h (the electrodialysis time T3 satisfied the above formula T3=(1 / 3+N)·C V ·V3·F / (I3·n3·η3)), the alkali chamber product was filtered to obtain vanadium hydroxide (V(OH)3) precipitate and a very small amount of vanadyl hydroxide (VO(OH)2) precipitate, which was weighed to 100.78g after vacuum drying (all products were regarded as vanadium hydroxide), and the comprehensive yield of vanadium hydroxide was 97.42%;

[0120] S3: Add 175 mL of concentrated hydrochloric acid to 0.1 L of water to obtain a dilute hydrochloric acid solution, dissolve 75.75 g of vanadium hydroxide (VO(OH)2) obtained in S2-1 in the dilute hydrochloric acid solution, stir and react for 30 minutes, add water to make the volume to 0.3 L, and obtain a hydrochloric acid-based positive electrode vanadium electrolyte product with a vanadium element concentration of 2.5 mol / L, a chloride ion concentration of 7.0 mol / L, and a vanadium element valence of +4; take 175 mL of concentrated hydrochloric acid and dilute it in 0.1 L of pure water to obtain a dilute hydrochloric acid solution, take 76.50 g of vanadium hydroxide (V(OH)3) obtained in S2-2 and dissolve it in the dilute hydrochloric acid solution, stir and react for 30 minutes, add water to make the volume to 0.3 L, and obtain a hydrochloric acid-based negative electrode vanadium electrolyte product with a vanadium element concentration of 2.5 mol / L, a chloride ion concentration of 7.0 mol / L, and a vanadium element valence of +3.

[0121] Test the performance of vanadium electrolyte: Assemble a single test vanadium battery using graphite electrode, flexible graphite plate and Nafion membrane as materials, and inject 100mL of the above products +4-valent electrolyte and +3-valent electrolyte into the effective area of ​​48cm 2 In the positive and negative electrodes of the vanadium battery, at 150mA / cm 2The constant current charge and discharge test was conducted for 50 cycles at a current density of 1.55V for charging and 1V for discharging. The test results are as follows: Figure 4 As shown, the battery operates normally with an energy efficiency of 82.57% on average.

[0122] Comparative Example 1

[0123] 23.42 g of low-purity ammonium polyvanadate (burning rate 78.4%, burnt purity 99.1%) obtained by extracting vanadium from vanadium slag from a factory in Xinjiang, which is the same as in Example 3, and 50.40 g of oxalic acid dihydrate were added to 0.2 L of water, heated to 35° C. under stirring conditions and maintained at the temperature for 60 min. After the reaction was completed, it was filtered and a large amount of undissolved solids were found. The vanadium concentration of the solution was measured to be 0.540 mol / L, and the yield was only 54.0%.

[0124] In this comparative example, since the reaction temperature during the dissolution reduction and impurity removal process is relatively low, the total vanadium concentration and yield of the product are low, and the utilization rate of ammonium polyvanadate is greatly reduced.

[0125] Comparative Example 2

[0126] Weigh 23.42 g of low-purity ammonium polyvanadate (burning rate 78.4%, burnt purity 99.1%) obtained by extracting vanadium from vanadium slag from a factory in Xinjiang, which is the same as in Example 3, and 50.40 g of oxalic acid dihydrate, add them to 0.2 L of water, heat to 60° C. under stirring conditions and maintain the temperature for 35 min. After the reaction is completed, filter the solution and measure the vanadium concentration of the solution to be 0.934 mol / L, with a yield of 93.4%.

[0127] In this comparative example, since the reaction time in the dissolution reduction and impurity removal process is not long enough, the total vanadium concentration and yield of the product are slightly low, and the utilization rate of ammonium polyvanadate is also slightly reduced.

Claims

1. A method for preparing a vanadium electrolyte, characterized in that: The method comprises the following steps S1, one or two steps selected from step S2-1 and step S2-2, and step S3: S1: low-purity ammonium vanadate, oxalic acid and water are mixed evenly, reacted, and filtered after the reaction is completed to obtain a first solution; wherein the low-purity ammonium vanadate is low-purity ammonium metavanadate or low-purity ammonium polyvanadate, the calcined purity of the low-purity ammonium vanadate is ≤99.5%, and all vanadium elements in the first solution are in the form of VO 2+ exists in the form of; S2-1: sending part or all of the first solution obtained in step S1 to the salt chamber of a first bipolar membrane electrodialysis device for electrodialysis, filtering and drying the product in the alkali chamber of the first bipolar membrane electrodialysis device to obtain a first intermediate product, wherein the first intermediate product is VO(OH)2; S2-2: sending part or all of the first solution obtained in step S1 to the cathode cell of an electrolysis device for electrolysis to obtain a second solution, wherein the average valence of the vanadium element in the second solution is +3.00 to +3.03, sending the second solution to the salt chamber of a second bipolar membrane electrodialysis device for electrodialysis, filtering and drying the product in the alkali chamber of the second bipolar membrane electrodialysis device to obtain a second intermediate product, wherein the second intermediate product is V(OH)3 and possibly VO(OH)2; S3: Dissolve the first intermediate product obtained in step S2-1 alone in an acid solution, or dissolve the second intermediate product obtained in step S2-2 alone in an acid solution, or dissolve the first intermediate product obtained in step S2-1 and the second intermediate product obtained in step S2-2 together in an acid solution to obtain a vanadium electrolyte in which the average valence of the vanadium element is +4, +3, or between +4 and +3.

2. The method according to claim 1, characterized in that In step S1, when the low-purity ammonium vanadate is low-purity ammonium metavanadate, low-purity ammonium metavanadate and oxalic acid are added according to a molar ratio of vanadium element to oxalic acid of 1:(2.2-2.5); In step S1, when the low-purity ammonium vanadate is low-purity ammonium polyvanadate, the low-purity ammonium polyvanadate and oxalic acid are added according to the molar ratio of vanadium element to oxalic acid of 3:(5.5-6.0).

3. The method according to claim 1, characterized in that The concentration of vanadium element in the reaction system in step S1 is 0.5 mol / L to 1.0 mol / L.

4. The method according to claim 1, characterized in that The reaction in step S1 is carried out under stirring at a reaction temperature of 50°C to 60°C.

5. The method according to claim 1, characterized in that When the low-purity ammonium vanadate used in step S1 is low-purity ammonium metavanadate, the electrodialysis time in step S2-1 is controlled as follows: T1 = 5·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C V is the vanadium concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device; When the low-purity ammonium vanadate used in step S1 is low-purity ammonium polyvanadate, the electrodialysis time in step S2-1 is controlled as follows: T1 = 13 / 3·C V ·V1·F / (I1·n1·η1), where T1 is the electrodialysis time in seconds; C V is the vanadium element concentration of the first solution entering the first bipolar membrane electrodialysis device, in mol / L; V1 is the volume of the first solution entering the first bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I1 is the electrolysis current of the first bipolar membrane electrodialysis device, in A; n1 is the number of electrodialysis units of the first bipolar membrane electrodialysis device; η1 is the current efficiency of the first bipolar membrane electrodialysis device.

6. The method according to claim 1, characterized in that The electrolysis time of the electrolysis device in step S2-2 is controlled as follows: T2 = C V ·V2·F / (I2·n2·η2), where T2 is the electrolysis time of the electrolysis device, in seconds; C V is the vanadium concentration of the first solution entering the electrolysis device, in mol / L; V2 is the volume of the first solution entering the electrolysis device, in L; F is the Faraday constant, which is 96485C / mol; I2 is the electrolysis current of the electrolysis device, in A; n2 is the number of electrolysis units of the electrolysis device; η2 is the current efficiency of the electrolysis device; When the low-purity ammonium vanadate used in step S1 is low-purity ammonium metavanadate, the electrodialysis time in step S2-2 is controlled as follows: T3 = (1 + N)·C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C V is the vanadium concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device; When the low-purity ammonium vanadate used in step S1 is low-purity ammonium polyvanadate, the electrodialysis time in step S2-2 is controlled as follows: T3 = (1 / 3 + N)·C V ·V3·F / (I3·n3·η3), where T3 is the electrodialysis time in seconds; N is the average valence of vanadium in the second solution entering the second bipolar membrane electrodialysis device; C V is the vanadium element concentration of the second solution entering the second bipolar membrane electrodialysis device, in mol / L; V3 is the volume of the second solution entering the second bipolar membrane electrodialysis device, in L; F is the Faraday constant, which is 96485C / mol; I3 is the electrolysis current of the second bipolar membrane electrodialysis device, in A; n3 is the number of electrolysis units of the second bipolar membrane electrodialysis device; η3 is the current efficiency of the second bipolar membrane electrodialysis device.

7. The method according to claim 1, characterized in that The first bipolar membrane electrodialysis device and the second bipolar membrane electrodialysis device each independently comprise an electrolysis unit or a plurality of electrolysis units connected in series, each electrolysis unit comprises a bipolar membrane, an acid chamber, an anion membrane, a salt chamber, an cation membrane, an alkali chamber and a bipolar membrane, the acid chamber is located between the bipolar membrane and the anion membrane, the salt chamber is located between the anion membrane and the cation membrane, and the alkali chamber is located between the cation membrane and the bipolar membrane; the electrodialysis process adopts a DC power supply, and the current density is 30 mA / cm 2 ~50mA / cm 2 ; The electrolysis device comprises one or more electrolysis units, each of which comprises a cathode plate, a cathode electrode, a cathode pool, a diaphragm, an anode pool and an anode plate. The cathode plate is made of graphite, the cathode electrode is made of carbon felt or graphite felt, the anode plate is made of titanium, the anode electrolyte is a sulfuric acid solution, and the current density of the electrolysis process is 80 mA / cm 2 ~120mA / cm 2 .

8. The method according to claim 1, characterized in that The method further comprises: in step S2-1, recycling the product in the acid chamber of the first bipolar membrane electrodialysis device to step S1, concentrating the product in the salt chamber of the first bipolar membrane electrodialysis device through a reverse osmosis system and recycling it as a raw material for the salt chamber of the first bipolar membrane electrodialysis device, recycling the water produced by the reverse osmosis system as an ion receiving liquid to the alkali chamber and / or the acid chamber of the first bipolar membrane electrodialysis device; and / or The method also includes: in step S2-2, the product in the acid chamber of the second bipolar membrane electrodialysis device is recycled to step S1, the product in the salt chamber of the second bipolar membrane electrodialysis device is concentrated by a reverse osmosis system and then recycled as a raw material for the salt chamber of the second bipolar membrane electrodialysis device, and the water generated by the reverse osmosis system is recycled as an ion receiving liquid to the alkali chamber and / or acid chamber of the second bipolar membrane electrodialysis device.

9. The method according to claim 1, characterized in that The acid solution in step S3 is a sulfuric acid solution, a hydrochloric acid solution or a mixture of the two.

10. The method according to claim 9, characterized in that When the acid solution in step S3 is a sulfuric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 2.0 mol / L, and the concentration of sulfate ions is 3 mol / L to 5.5 mol / L; When the acid solution in step S3 is a hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 4.0 mol / L, and the concentration of chloride ions is 6 mol / L to 8 mol / L; When the acid solution in step S3 is a mixture of sulfuric acid solution and hydrochloric acid solution, the concentration of vanadium element in the vanadium electrolyte is 1.5 mol / L to 3.5 mol / L, the concentration of sulfate ions is 1 mol / L to 3.0 mol / L, and the concentration of chloride ions is 3 mol / L to 6 mol / L.

Citation Information

Cited By

  • Method for directly preparing vanadium battery electrolyte from vanadium liquid without participation of organic matters

    CN120809897A

  • Method for directly preparing vanadium battery electrolyte from vanadium solution without organic participation