Substrate processing method, LED chip substrate and LED product
By using mask production, main etching and over-etching steps to form a conical etching pattern on the sapphire substrate, combined with the by-product removal step, the problem of insufficient flatness of the substrate surface is solved, and the quality and quality of the epitaxial layer are improved. LED chip performance.
Patent Information
- Application Number
- CN202310339703.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-31
AI Technical Summary
During the epitaxy process of LED chips, the surface of the sapphire substrate is not flat enough, resulting in poor quality of the epitaxial layer and affecting product performance.
A substrate processing method is adopted, including mask production, main etching and over-etching steps, and a conical etching pattern is formed by patterning the mask layer and plasma etching, combined with a by-product removal step, to ensure that the substrate surface Flatness.
It improves the flatness of the substrate surface, improves the quality of the epitaxial layer and the performance of semiconductor products, and ensures the efficient production of LED chips.
Smart Images

Figure CN118738244A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of semiconductor processing technology, and specifically relates to a substrate processing method, an LED chip substrate and an LED product. Background Art
[0002] As the mainstream substrate application material in the field of LED chips, sapphire substrate can effectively reduce the dislocation density generated by the epitaxial layer and reduce epitaxial defects, thereby significantly improving the crystal quality of the epitaxial layer and further improving product performance. In the epitaxial process of LED chips, an aluminum nitride layer is usually deposited on the surface of the substrate to provide a base, and then a gallium nitride layer is deposited on the surface of the aluminum nitride layer. The flatness of the substrate surface is closely related to the epitaxial quality. Therefore, how to form a substrate with a flat surface is a problem that needs to be solved urgently. Summary of the invention
[0003] The purpose of the embodiments of the present application is to provide a substrate processing method, an LED chip substrate and an LED product. The substrate processing method can be used to form a substrate with a relatively flat surface.
[0004] In a first aspect, an embodiment of the present application discloses a substrate processing method, the substrate processing method comprising:
[0005] A mask making step, covering the upper surface of the substrate with a patterned mask layer to form a piece to be etched; wherein the substrate is a sapphire substrate, and the patterned mask layer includes a plurality of cylindrical mask structures that are spaced apart from each other and distributed in a determinant;
[0006] A main etching step, etching the to-be-etched piece while the process chamber is kept under the first process condition to form an intermediate piece;
[0007] an over-etching step, in which the intermediate member is etched while the process chamber is maintained at a third process condition to form a patterned substrate, wherein the patterned substrate comprises a plurality of conical structure etching patterns that are spaced from each other and distributed in a matrix;
[0008] After the main etching step is completed once, at least one by-product removal step is performed, and / or, after the over-etching step is completed once, at least one by-product removal step is performed;
[0009] The byproduct removal step includes bombarding the etching byproducts on the surface of the to-be-etched object while the process chamber maintains a second process condition, wherein the second process gas in the second process condition is an inert gas.
[0010] In a second aspect, an embodiment of the present application discloses an LED chip substrate, which is formed by the above-mentioned substrate processing method, wherein the LED chip substrate comprises a base and a plurality of etching patterns protruding from the upper surface of the base, the upper surface of the base is a plane, the plurality of etching patterns are spaced from each other and are distributed in a determinant, and each of the etching patterns is a conical structure.
[0011] In a third aspect, an embodiment of the present application discloses an LED product, which includes an epitaxial layer and the above-mentioned LED chip substrate, wherein the epitaxial layer covers the upper surface of the LED chip substrate.
[0012] The embodiment of the present application discloses a substrate processing method, which first covers the upper surface of the substrate with a patterned mask layer to provide a masking effect for the etching pattern formed on the substrate to achieve pattern transfer. In addition, the patterned mask layer includes a plurality of cylindrical mask structures that are spaced apart from each other and distributed in a determinant, so that in the subsequent etching process, the plasma can enter the gap between the mask structures to etch the sidewalls of the mask structures, and the gap between the mask structures is limited to a single-side opening structure, so that the etching rate of the part of the sidewall of the mask structure that is farther away from the lower surface of the substrate is greater, and as the etching process continues, the pattern in the pattern transfer function provided by the cylindrical mask structure to the substrate finally presents a conical shape, so that the patterned substrate includes a base and a plurality of conical etching patterns, and the plurality of etching patterns are spaced apart from each other and distributed in a determinant.
[0013] Furthermore, during the processing, the main etching step and the over-etching step are respectively performed on the workpiece to be etched. Specifically, the process chamber is maintained at the first process condition and the third process condition respectively to etch the workpiece to be etched. At the same time, compared with the main etching step, the power of the lower electrode is relatively larger during the over-etching step, which makes the kinetic energy of the plasma generated by the process gas in the third process condition relatively larger, which is beneficial to gradually remove the edges and corners of the etching pattern in the intermediate part, so that the etching pattern gradually approaches the ideal conical structure.
[0014] In addition, by performing at least one by-product removal step after completing the main etching step once, and / or performing at least one by-product removal step after completing the over-etching step once, the second process gas in the second process condition can bombard the by-products on the surface of the etched part, thereby preventing the by-products generated during the etching process from affecting the uniformity of the etching process, and making the surface of the etched part as flat as possible, so that the surface of the patterned substrate formed by the substrate processing method disclosed in the embodiment of the present application can be a relatively flat structure, so that when the patterned substrate is used for the epitaxial process, the formation quality of the epitaxial layer can be guaranteed to be relatively high, thereby improving the product quality of the semiconductor. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0016] Figure 1 It is an electron microscope photograph of the etched part after only the main etching step is performed;
[0017] Figure 2 for Figure 1 Electron microscope photograph of the formed part to be etched after only the etching step is performed;
[0018] Figure 3 A schematic diagram of a process flow of a substrate processing method disclosed in an embodiment of the present application;
[0019] Figure 4 This is an electron microscope photograph of an intermediate piece formed in the substrate processing method disclosed in the embodiment of the present application;
[0020] Figure 5 This is an electron microscope photograph of a patterned substrate formed in the substrate processing method disclosed in the embodiment of the present application. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0022] The terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described here, and the objects distinguished by "first", "second", etc. are generally of one type, and the number of objects is not limited. For example, the first object can be one or more. In addition, "and / or" in the specification and claims represents at least one of the connected objects, and the character " / " generally indicates that the objects associated with each other are in an "or" relationship.
[0023] As described above, the technical problem to be solved by the present application is how to form a substrate with a relatively flat surface. Based on the research on the above technical problem, the inventors found that a patterned sapphire substrate can be formed by sequentially performing a main etching step and an over-etching step. The by-products generated during the etching process will be deposited on the surface of the substrate. Although the by-products will be re-etched to be removed by the etching effect, the deposition distribution of the by-products is highly random, resulting in different thicknesses of the by-products deposited at different positions on the substrate surface. Figure 1 and Figure 2 As shown, as the etching time continues to increase, the etching depths at different locations on the substrate surface differ, which causes the surface of the substrate to be uneven, which can have a serious adverse effect on the quality of the subsequent epitaxial process.
[0024] Based on the above situation, the inventors have made further improvements to the processing technology of the substrate, such as Figure 3 , and combined Figure 4 and Figure 5 An embodiment of the present application discloses a substrate processing method. By using the substrate processing method, a substrate can be processed so that the substrate can be patterned to form a patterned substrate, wherein the substrate is specifically a sapphire substrate.
[0025] In detail, the substrate processing method includes:
[0026] S1, mask making step, covering the upper surface of the substrate with a patterned mask layer to form a part to be etched. That is, in the present application, the part to be etched includes a substrate and a patterned mask layer, both of which are etched together. Optionally, the patterned mask layer can be formed by coating, or it can also be formed by embossing, that is, the patterned mask layer is an embossed adhesive mask.
[0027] Moreover, in the substrate processing method disclosed in the embodiment of the present application, the processed substrate is a sapphire substrate. When such a substrate is used to form an LED chip, the dislocation density generated in the epitaxial layer can be effectively reduced, and the epitaxial quality can be improved. Accordingly, in order to form the desired pattern on the substrate, it is necessary to make the patterned mask layer have a corresponding pattern. In detail, the patterned mask layer includes a plurality of cylindrical mask structures, and the plurality of mask structures are spaced apart from each other and distributed in a matrix, thereby ensuring that the subsequent etching process can form an etching pattern spaced apart from each other and distributed in a matrix on the substrate. Specifically, dimensions such as the diameter and thickness of the mask structure, as well as parameters such as the spacing between two adjacent mask structures, can be flexibly determined according to actual needs and are not limited here.
[0028] In a specific embodiment, a patterned mask layer may be formed by coating a photoresist. Specifically, the above step S1 may include:
[0029] The photoresist is coated on the upper surface of the substrate to form a photoresist layer. Specifically, the photoresist with a preset thickness can be coated on the upper surface of the substrate by spin coating or the like to form a photoresist layer on the upper surface of the substrate.
[0030] Afterwards, the photoresist layer is processed by exposure and development, so that the part of the photoresist layer that needs to be used as a mask is retained, and the other parts of the photoresist layer except for the mask are removed to form a patterned photoresist layer. Accordingly, the patterned photoresist layer includes multiple cylindrical mask structures that are spaced apart from each other and distributed in a matrix.
[0031] Specifically, the thickness of the photoresist layer may be between 2.0 μm and 3.0 μm, and in each row and column of cylindrical mask structures, the distance between the centers of any two adjacent mask structures may be 3.0 μm, and the diameter of the mask structure may be between 2.0 μm and 2.3 μm.
[0032] After the above step S1, the substrate processing method disclosed in the embodiment of the present application further includes:
[0033] S2, a main etching step, etching the workpiece to be etched to form an intermediate workpiece while maintaining the first process condition in the process chamber.
[0034] In the first process condition, the process gas introduced into the process chamber is the first process gas, and the first process gas is used to generate a first plasma to etch the object to be etched. That is, when the process chamber maintains the first process condition, an etching process is performed in the process chamber to etch the object to be etched from the upper surface of the object to be etched.
[0035] Furthermore, in the aforementioned etching process, since a patterned mask layer is provided on the upper surface of the substrate, and the mask structures included in the patterned mask are spaced apart from each other, during the process of etching the etched part using the first process gas, the first plasma can not only etch the upper surface of the etched part (including the mask structure and the substrate), but can also etch the side walls of the mask structure by moving to the gap between any two adjacent mask structures.
[0036] At the same time, since the etching process will produce by-products, for the etching process of the side wall of the mask structure, the by-products produced after the area of the side wall closer to the upper surface is etched are easier to be discharged from the gap, and the first plasma is easier to enter the area of the mask structure closer to the upper surface. Therefore, the etching rate of the area of the side wall of the mask structure closer to the upper surface is greater.
[0037] On the contrary, since the first plasma is less likely to enter the area closer to the bottom in the gap between the mask structures, and the byproducts generated by the etching process are not easily discharged from the bottom of the mask structure, the etching rate of the part closer to the bottom of the side wall of the mask structure is also lower. Furthermore, as the etching process continues, the shape of the cylindrical mask structure will change to a structure with a small top and a large bottom, and the difference between the diameter of the lower surface and the diameter of the upper surface of the mask structure will become larger and larger, thereby ensuring that as the processing process continues, the mask structure will change the shape of the transferred pattern while providing the substrate with a pattern transfer function, and finally form a plurality of mutually spaced and determinant-distributed conical etching patterns on the upper half of the substrate.
[0038] Specifically, the first process gas can generate plasma that can react with the etched part (including the sapphire substrate and the mask layer). Since the mask layer is usually a glue layer, it is relatively easy to etch and remove, and there is almost no need to consider the type of gas used to etch the mask layer separately. Since the main component of the sapphire substrate is aluminum oxide, for this reason, the first process gas can include boron chloride, and the ions generated after it is ionized are easy to react with aluminum oxide, and the generated by-products are mostly gaseous materials, which can reduce the difficulty of controlling the etching work. Of course, the first process gas can be a single-component gas, or it can also be formed by mixing two or more gases.
[0039] Based on this, in order to improve the etching efficiency and etching effect, the first process gas may also include trifluoromethane. That is, the first process gas includes boron chloride and trifluoromethane. In this case, after the first process gas is introduced into the process chamber, the reactions that occur include:
[0040] BCl3↑→BCl x +↓+Cl-↑(x=0,1,2);
[0041] Al2O3↓+BCl x +↑→Al3+↑+BOCl z +↑+Cl-↑(z=1,2,3);
[0042] Cl-↑+Al3+↑→AlCl3↓;
[0043] CHF3↑→CHF m +↑+F-↑(m=0,1,2);
[0044] Al3+↑+F-↑→AlF3↓;
[0045] Of course, when the first process gas includes boron chloride, it may also include hydrogen and dichloromethane, etc., but does not include trifluoromethane. The assembly methods of these first process gases can ensure that the etched part can be etched normally. In general, the first process gas includes boron chloride, or the first process gas includes boron chloride, and the first process gas also includes at least one of trifluoromethane, hydrogen and dichloromethane.
[0046] After the above step S2, a part of the etched part can be etched away to form an intermediate part. For this purpose, compared with the etched part, the substrate of the intermediate part has an etching groove, and the etching groove corresponds to the gap between the mask structures in the patterned mask layer, and the size of the mask structure in the intermediate part becomes smaller. At the same time, the diameter of the upper surface of the mask structure is smaller than the diameter of the lower surface, that is, the mask structure is small at the top and large at the bottom.
[0047] After the above step S2, the intermediate piece formed after the etched piece through the above step S2 needs to be further processed to form the patterned substrate required by the present application. Based on this, the substrate processing method disclosed in the above embodiment of the present application also includes:
[0048] S3, an over-etching step, while the process chamber maintains the third process condition, etching the intermediate piece to form a patterned substrate, corresponding to the above-mentioned patterned mask layer, and based on the etching principle, the patterned substrate formed after completing the over-etching step includes a plurality of conical structure etching patterns that are spaced from each other and distributed in a matrix.
[0049] In the third process condition, the process gas introduced into the process chamber is a third process gas, and the third process gas is used to generate a third plasma to etch the intermediate component. That is, when the process chamber maintains the third process condition, the process performed in the process chamber also belongs to the etching process, and the intermediate component is etched from the upper surface of the intermediate component.
[0050] Furthermore, in the initial stage of the aforementioned etching process, since part of the mask layer may still exist on the upper surface of the substrate, and the mask structures are spaced apart from each other, the substrate has an etching groove, and then in the process of etching the intermediate member using the third process gas, the sidewalls of the etching groove in the substrate can be further etched to expand the width of the etching groove. Furthermore, as the etching process continues, the mask layer can be completely etched away, so that the depth of the etching groove on the substrate continues to increase, and the width of the etching groove farther from the bottom surface of the substrate is larger, and the width of the part closer to the bottom surface of the substrate is smaller, so as to ensure that the patterned substrate includes a plurality of conical etching patterns that correspond to the mask structures, are spaced apart from each other, and are distributed in a determinant.
[0051] Optionally, similar to the first process gas, the third process gas may include boron chloride to reduce the difficulty of etching control of the intermediate component. Of course, when the third process gas includes boron chloride, in order to improve the etching efficiency, the third process gas may also include at least one of trifluoromethane, hydrogen and dichloromethane, which is not limited herein.
[0052] In addition, it is necessary to make the lower electrode power in the third process condition greater than the lower electrode power in the first process condition, so that the kinetic energy of the plasma during the etching process in step S3 is greater than the kinetic energy of the corresponding plasma during the etching process in step S2. This makes the plasma in step S3 have a relatively stronger etching effect, so that the corners and edges of the etching pattern can be gradually removed in step S3, thereby making the etching pattern tend to a more ideal cone shape.
[0053] After the above step S3, the remaining mask layer on the intermediate part can be completely removed, and the depth and width of the etched grooves on the intermediate part can be further expanded, thereby forming a patterned substrate. More specifically, the patterned substrate includes a substrate and a plurality of etching patterns protruding from the upper surface of the substrate. The upper surface of the substrate is a plane, and the plurality of etching patterns are spaced from each other and distributed in a determinant, and each etching pattern is a conical structure. It should be noted that the upper surface of the substrate is the internal structure of the substrate before etching. By forming etching grooves on the substrate, part of the internal structure of the substrate is exposed, thereby forming a "new upper surface", that is, the upper surface of the substrate; and the substrate and the plurality of etching patterns are an integrated structure. In the present application, in order to distinguish the functional parts in the patterned substrate, it is artificially divided into two structures. In fact, there is no obvious boundary between the two structures in structure.
[0054] Furthermore, in order to ensure that the surface of the substrate formed through the above steps S2 and S3 is relatively flat, the substrate processing method disclosed in the embodiment of the present application further includes:
[0055] S4, after completing the main etching step once, performing at least one byproduct removal step, and / or performing at least one byproduct removal step after completing the over-etching step once. The byproduct removal step includes: bombarding the etching byproducts on the surface of the to-be-etched part under the condition that the process chamber maintains the second process condition, and the second gas in the second process condition is an inert gas.
[0056] As for the second process gas, it is mainly used to bombard the etched part to remove the byproducts on the surface of the etched part. To this end, it is necessary to ensure that the second process gas cannot react with the etched part. Based on this, as mentioned above, the second process gas is an inert gas. Optionally, the second process gas includes argon gas to reduce production costs while meeting the needs. Correspondingly, after the second process gas is introduced into the process chamber, the reactions generated include:
[0057] Ar↑→Ar+↑+e-;
[0058] Of course, the second process gas may also include neon gas or krypton gas.
[0059] After the second process gas is introduced into the process chamber, it can be ionized to generate ions, and under the action of the lower electrode power, it moves in the direction close to the etched part, and finally collides with the etched part to remove the etching by-products on the surface of the etched part by bombardment. Since the substrate selected in the embodiment of the present application is a sapphire substrate, its hardness is relatively large and its bombardment resistance is strong. Therefore, in the process of bombarding the etched part with the second process gas to remove the etching by-products, the sapphire substrate will hardly be damaged. Of course, in order to further prevent the sapphire substrate from being damaged by the second plasma, the lower electrode power can be controlled accordingly according to the actual process, so that the second plasma has the ability to remove the etching by-products while not damaging the sapphire substrate.
[0060] As described above, the by-product removal step can be performed at least once after the main etching step is completed once. In this case, the process chamber can switch the process conditions from the first process conditions to the second process conditions after completing the main etching step once. Of course, there may be some process parameters that are the same in the two process conditions, or any of the process parameters in the two process conditions may be different.
[0061] In a specific embodiment of the present application, the time for a single main etching step can be 60-120s, and the time for a single by-product removal step can be 30-60s. Based on this, the process chamber can be switched to maintaining the second process condition for 30-60s after maintaining the first process condition for 60-120s, so that the by-products generated by the substrate during the etching process and attached to its surface can be removed with the help of the by-product removal step, thereby preventing the by-products from affecting the subsequent etching process, thereby allowing the surface of the etched part to always remain in a relatively flat state.
[0062] Furthermore, the main etching step and the by-product removal step can be performed alternately, that is, the process chamber is alternately cycled to maintain the first process condition and the second process condition to provide a corresponding process environment for the etched parts located in the process chamber, and the holding time of the first process condition and the second process condition can be determined according to actual conditions.
[0063] When adopting the above scheme, if Figure 4As shown, while ensuring that the surface of the intermediate piece formed after the main etching step has a relatively flat surface, a high etching efficiency can also be taken into account. Accordingly, by making the process chamber alternately cycle and maintain the first process condition and the second process condition for multiple times, the piece to be etched can be etched and the intermediate piece can be formed. The number of alternations of the two process conditions can be determined according to actual conditions, and can be specifically 10 to 20 times, which can further take into account both etching efficiency and etching effect.
[0064] When at least one by-product removal step is performed after a single main etching step is completed, the total time of the main etching step can be controlled to determine the timing of completing the main etching step. Alternatively, the etching depth of the groove on the intermediate part can be used as a reference to determine the timing of completing the main etching step.
[0065] More specifically, as described above, a patterned mask layer can be formed using photoresist, and the thickness of the photoresist layer is 2.0 μm to 3.0 μm. In this case, when the depth of the etched groove on the intermediate member ranges from 1.2 to 1.7 μm, it can be considered that the main etching step can be terminated at this time.
[0066] As described above, the by-product removal step can also be performed at least once after a single over-etching step is completed. In this case, the process chamber can switch the process conditions from the third process conditions to the second process conditions after completing one over-etching step. Of course, some process parameters may be the same in the two process conditions, or any of the process parameters may be different.
[0067] In a specific embodiment of the present application, the time for a single over-etching step can be 60-120 seconds, and the time for a single by-product removal step can be 30-60 seconds. Based on this, the process chamber can be switched to maintaining the second process condition for 30-60 seconds after maintaining the third process condition for 60-120 seconds, thereby removing the by-products generated on the substrate and attached to its surface during the etching process with the help of the by-product removal step.
[0068] Furthermore, the over-etching step and the by-product removal step can be performed alternately, that is, the process chamber is alternately cycled to maintain the third process condition and the second process condition, the intermediate member can be etched to form a patterned substrate, and as Figure 5 As shown, the surface of the formed patterned substrate is ensured to be relatively smooth and flat. The number of alternations of the two process conditions can be determined according to actual conditions, and can be specifically 5 to 10 times, so as to take into account both etching effect and etching efficiency.
[0069] Accordingly, the completion timing of the over-etching step can be determined based on the morphology of the etching pattern in the etched substrate. Specifically, as described above, a patterned mask layer can be formed using photoresist so that the thickness of the photoresist layer is 2.0μm to 3.0μm, and when the above-mentioned main etching step is completed, the depth of the etched groove on the intermediate piece is in the range of 1.2μm-1.7μm. In this case, when the intermediate piece is processed into the substrate so that the etching pattern protruding from the upper surface is cone-shaped as a whole, and its height is 1.6μm-1.9μm, and the bottom width is 2.6μm-2.9μm, it can be considered that a patterned substrate has been formed, and the over-etching step can be terminated at this time.
[0070] The embodiment of the present application discloses a substrate processing method, which first covers the upper surface of the substrate with a patterned mask layer to provide a masking effect for the etching pattern formed on the substrate to achieve pattern transfer. In addition, the patterned mask layer includes a plurality of cylindrical mask structures that are spaced apart from each other and distributed in a determinant, so that in the subsequent etching process, the plasma can enter the gap between the mask structures to etch the sidewalls of the mask structures, and the gap between the mask structures is limited to a single-side opening structure, so that the etching rate of the part of the sidewall of the mask structure that is farther away from the lower surface of the substrate is greater, and as the etching process continues, the pattern in the pattern transfer function provided by the cylindrical mask structure to the substrate finally presents a conical shape, so that the patterned substrate includes a base and a plurality of conical etching patterns, and the plurality of etching patterns are spaced apart from each other and distributed in a determinant.
[0071] Furthermore, during the processing, the main etching step and the over-etching step are respectively performed on the workpiece to be etched. Specifically, the process chamber is maintained at the first process condition and the third process condition respectively to etch the workpiece to be etched. At the same time, compared with the main etching step, the power of the lower electrode is relatively larger during the over-etching step, which makes the kinetic energy of the plasma generated by the process gas in the third process condition relatively larger, which is beneficial to gradually remove the edges and corners of the etching pattern in the intermediate part, so that the etching pattern gradually approaches the ideal conical structure.
[0072] In addition, by performing at least one by-product removal step after completing the main etching step once, and / or performing at least one by-product removal step after completing the over-etching step once, the second process gas in the second process condition can bombard the by-products on the surface of the etched part, thereby preventing the by-products generated during the etching process from affecting the uniformity of the etching process, and making the surface of the etched part as flat as possible, so that the surface of the patterned substrate formed by the substrate processing method disclosed in the embodiment of the present application can be a relatively flat structure, so that when the patterned substrate is used for the epitaxial process, the formation quality of the epitaxial layer can be guaranteed to be relatively high, thereby improving the product quality of the semiconductor.
[0073] In the above embodiment, the etched part and the intermediate part are both located in the process chamber, and in the process of processing the two, the process chamber is set with corresponding process conditions, which generally include chamber pressure, upper electrode power, lower electrode power, gas type and corresponding flow rate, etc. Of course, in order to ensure that the temperature of the etched part and the intermediate part will not be relatively high during the etching process, helium can also be introduced under the etched part to provide a cooling effect for it, and the pressure of helium can be 3-7Torr. In addition, a cooler can be provided to provide a further cooling effect for the etched part, and the setting temperature of the cooler can be 0-40°C.
[0074] During the processing of the substrate, various parameters in the process conditions in the process chamber can be comprehensively considered. Optionally, in the first process condition, the pressure range of the process chamber can be 2-3mTorr, the upper electrode power range can be 1200-2000W, the lower electrode power range can be 300-600W, the first process gas can include boron chloride and trifluoromethane, and the flow rate of boron chloride can be 100-150sccm, and the flow rate of trifluoromethane can be 5-20sccm. When the above process formula is adopted, the etching efficiency and etching effect of the etched part are relatively high.
[0075] Optionally, in the second process condition, the pressure range of the process chamber can be 2-3mTorr, the upper electrode power range can be 1200-2000W, the lower electrode power range can be 50-200W, and the second process gas can include argon, and its flow rate can be 50-100sccm, which makes the removal of etching by-products relatively thorough and efficient, and will not damage the substrate.
[0076] Optionally, in the third process condition, the pressure range of the process chamber can be 2-3mTorr, the power range of the upper electrode can be 1200-2000W, the power range of the lower electrode can be 700-1000W, the third process gas can include boron chloride and trifluoromethane, the flow rate of boron chloride can be 60-120sccm, and the flow rate of trifluoromethane can be 3-10sccm. When the above process formula is adopted, the etching efficiency and etching effect of the intermediate piece are relatively high, and it is conducive to forming an ideal conical structure of the etching pattern.
[0077] Based on the substrate processing method disclosed in any of the above embodiments, the embodiments of the present application also disclose an LED chip substrate, which is formed by the substrate processing method disclosed in any of the above embodiments, that is, the LED chip substrate is made of sapphire, and includes a base and a plurality of etching patterns protruding from the upper surface of the base, the upper surface of the base is a plane, and the plurality of etching patterns are spaced apart from each other, and at the same time, the plurality of etching patterns are distributed in a determinant, each etching pattern is a cone-shaped structure, and the surface of each etching pattern is relatively flat and smooth. More specifically, in the LED chip substrate, the shape and size of each etching pattern are basically the same, the height of the etching pattern is 1.6-1.9um, and the bottom width of the etching pattern is 2.6-2.9um. The substrate can provide an ideal growth platform for the epitaxial layer of the LED chip, and is suitable for MOCVD epitaxial growth of LED chips such as white light LED, blue light LED, green light LED, MiniLED, and MicroLED.
[0078] Based on the above LED chip substrate, the embodiment of the present application further discloses an LED product, which can be specifically an LED chip, and the LED product includes an epitaxial layer and the above LED chip substrate, and the epitaxial layer covers the upper surface of the LED chip substrate. Specifically, the epitaxial layer can be formed on the upper surface of the LED chip substrate by an epitaxial process, and the specific material of the epitaxial layer can be GaN.
[0079] More specifically, in the process of forming the epitaxial layer, a layer of AlN with a thickness of 1 to 20 nm can be deposited on the upper surface of the LED chip substrate to provide a base and reduce the difficulty of processing the epitaxial layer. After that, the GaN epitaxial layer is grown, and the thickness of the GaN epitaxial layer can be 4-5um. The GaN epitaxial layer will start from the bottom platform of the substrate and continue to grow in the vertical direction starting from the AlN surface, and finally obtain the required high-quality LED chip.
[0080] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0081] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A substrate processing method, characterized in that: The substrate processing method comprises: A mask making step, covering the upper surface of the substrate with a patterned mask layer to form a piece to be etched; wherein the substrate is a sapphire substrate, and the patterned mask layer includes a plurality of cylindrical mask structures that are spaced apart from each other and distributed in a determinant; A main etching step, etching the to-be-etched piece while the process chamber is kept under the first process condition to form an intermediate piece; an over-etching step, in which the intermediate member is etched while the process chamber is maintained at a third process condition to form a patterned substrate, wherein the patterned substrate comprises a plurality of conical structure etching patterns that are spaced from each other and distributed in a matrix; After completing the main etching step once, performing a byproduct removal step at least once, and / or performing a byproduct removal step at least once after completing the over-etching step once; wherein the byproduct removal step comprises: bombarding the etching byproducts on the surface of the workpiece to be etched while maintaining a second process condition in the process chamber, wherein the second process gas in the second process condition is an inert gas.
2. The substrate processing method according to claim 1, characterized in that: The main etching step and the by-product removal step are performed alternately; The process chamber maintains the first process condition for 60-120 seconds at a time, and the process chamber maintains the second process condition for 30-60 seconds at a time.
3. The substrate processing method according to claim 2, characterized in that: The main etching step and the by-product removal step are alternately performed for a number of times ranging from 10 to 20 times.
4. The substrate processing method according to any one of claims 1 to 3, characterized in that: The over-etching step and the by-product removing step are performed alternately; The process chamber maintains the third process condition for 60-120 seconds at a time, and the process chamber maintains the second process condition for 30-60 seconds at a time.
5. The substrate processing method according to claim 4, characterized in that: The over-etching step and the by-product removal step are alternately performed for a number of times ranging from 5 to 10 times.
6. The substrate processing method according to claim 1, characterized in that: The first process gas in the first process condition includes boron chloride, or the first process gas in the first process condition includes boron chloride and the first process gas further includes at least one of trifluoromethane, hydrogen and dichloromethane; The third process gas in the third process condition includes boron chloride, or the third process gas in the third process condition includes boron chloride and the third process gas further includes at least one of trifluoromethane, hydrogen and dichloromethane.
7. The substrate processing method according to claim 1, characterized in that: The second process gas includes at least one of argon, neon or krypton.
8. The substrate processing method according to claim 1, characterized in that: In the first process condition, the pressure range of the process chamber is 2-3mT, the power range of the upper electrode is 1200-2000W, the power range of the lower electrode is 300-600W, the first process gas includes boron chloride and trifluoromethane, the flow rate of boron chloride is 100-150sccm, and the flow rate of trifluoromethane is 5-20sccm; And / or, in the third process condition, the pressure range of the process chamber is 2-3mT, the power range of the upper electrode is 1200-2000W, the power range of the lower electrode is 700-1000W, the third process gas includes boron chloride and trifluoromethane, the flow rate of boron chloride is 60-120sccm, and the flow rate of trifluoromethane is 3-10sccm.
9. The substrate processing method according to claim 1, characterized in that: In the second process condition, the pressure range of the process chamber is 2-3 mT, the power range of the upper electrode is 1200-2000 W, the power range of the lower electrode is 50-200 W, and the second process gas includes argon gas, and its flow rate is 50-100 sccm.
10. An LED chip substrate, characterized in that: The LED chip substrate is formed by the substrate processing method according to any one of claims 1 to 9, wherein the LED chip substrate comprises a base and a plurality of etching patterns protruding from the upper surface of the base, the upper surface of the base is a plane, the plurality of etching patterns are spaced apart from each other and are distributed in a matrix, and each of the etching patterns is a conical structure.
11. The LED chip substrate according to claim 10, characterized in that: The height of the etched pattern is 1.6-1.9 um, and the bottom width of the etched pattern is 2.6-2.9 um.
12. An LED product, characterized in that: It comprises an epitaxial layer and the LED chip substrate according to claim 10 or 11, wherein the epitaxial layer covers the upper surface of the LED chip substrate.
Citation Information
Patent Citations
Method for manufacturing semiconductor light-emitting device
CN102412348A
Preparation method of patterned sapphire substrate
CN108321261A
Manufacturing method for patterned substrate, patterned substrate and light emitting diode
CN110867503A
Plasma etch processes
US20200273711A1