Aqueous phosphorus-carbon negative electrode slurry and preparation method thereof, phosphorus-carbon negative electrode and lithium ion battery

Through the preparation of aqueous phosphorus-carbon negative electrode slurry, the problems of single selection of negative electrode materials and insufficient battery performance of lithium-ion batteries are solved, a lithium-ion battery system with high energy density and fast charging safety is achieved, the production process is simplified and the cost is reduced. .

CN118738260APending Publication Date: 2024-10-01UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410943599.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have a single choice of negative electrode materials. The graphite negative electrode has a low specific capacity and is prone to lithium precipitation side reactions during high-current charging, causing thermal runaway of the battery and hindering the further development of lithium-ion batteries.

Method used

Water-based phosphorus-carbon negative electrode slurry is used, including phosphorus-carbon composite, binder, conductive agent and dispersant, and is prepared by shear flow method to form a stable water-based phosphorus-carbon negative electrode slurry, which is used for the pole piece coating of phosphorus-carbon negative electrodes. cloth to improve the lithium storage capacity, conductivity and structural stability of the negative electrode.

Benefits of technology

It achieves the high energy density and fast charging safety of lithium-ion batteries, improves the cycle stability and charge and discharge power density of the battery, simplifies the production process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738260A_ABST
    Figure CN118738260A_ABST
Patent Text Reader

Abstract

The invention provides water-based phosphorus-carbon negative electrode slurry and a preparation method thereof, a phosphorus-carbon negative electrode and a lithium ion battery, and belongs to the technical field of new energy storage. The water-based phosphorus-carbon negative electrode slurry comprises a phosphorus-carbon compound, a binder, a conductive agent, water and a dispersant, the phosphorus-carbon compound is an insoluble solid, the solid content of the slurry in the water-based phosphorus-carbon negative electrode slurry is 10-70 wt%, and the viscosity range of the water-based phosphorus-carbon negative electrode slurry is 2000-12000mPa. S; the dispersing agent comprises at least one of polyphosphate, polycarboxylate and polyether derivative. The components of the water-based phosphorus-carbon negative electrode slurry are designed, so that particles of a phosphorus-carbon compound are uniformly and stably dispersed in a water system, coagulation of the slurry is avoided, and the water-based phosphorus-carbon negative electrode slurry can be directly used for pole piece coating of a phosphorus-carbon negative electrode; and the subsequently assembled lithium ion battery has good rate capacity exertion and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy storage technology, and in particular to an aqueous phosphorus-carbon negative electrode slurry and a preparation method thereof, a phosphorus-carbon negative electrode, and a lithium ion battery. Background Art

[0002] In the field of new energy storage technology, lithium-ion batteries have the advantages of high energy density, high power density and good safety performance, and thus have become a more important power device in the current new energy passenger vehicle field. Currently, the negative electrode material selection of commercial lithium-ion batteries is relatively single, and graphite negative electrodes occupy the main market advantage. However, the specific capacity of graphite negative electrodes is low (372mAh / g), and lithium precipitation side reactions are prone to occur under high current charging conditions, causing thermal runaway of the battery. These problems have seriously hindered the further development of lithium-ion batteries.

[0003] Phosphorus-carbon anode is an emerging anode material. Due to its excellent properties such as high specific capacity (pure phosphorus 2596mAh / g), fast charging and safety (6-C charging), researchers believe that it is a candidate for the anode that is expected to realize the next generation of high energy density, fast charging and safety battery systems. The commercial application of phosphorus-carbon anodes currently faces two major production challenges: material preparation and battery manufacturing. It not only requires the realization of cheap and safe large-scale preparation technology, but also the completion of the full process exploration from materials to batteries.

[0004] In the battery manufacturing process, the preparation of negative electrode slurry has a great influence on the performance of the electrode and battery. It should not only be conducive to the performance of phosphorus-carbon materials, but also ensure the quality of the coating process. However, there are few reports on the research of phosphorus-carbon negative electrode slurry system, and this key technology still needs to be developed urgently. Summary of the invention

[0005] In view of this, in order to at least partially solve at least one of the above-mentioned technical problems, the present invention provides an aqueous phosphorus-carbon negative electrode slurry and a preparation method thereof, a phosphorus-carbon negative electrode, and a lithium-ion battery.

[0006] According to an embodiment of one aspect of the present invention, an aqueous phosphorus-carbon negative electrode slurry is provided, comprising: a phosphorus-carbon composite, a binder, a conductive agent, water and a dispersant, wherein the phosphorus-carbon composite is an insoluble solid, and in the aqueous phosphorus-carbon negative electrode slurry, the slurry solid content is 10-70wt%, and the viscosity of the aqueous phosphorus-carbon negative electrode slurry ranges from 2000 to 12000mPa·s; the dispersant comprises at least one of a polyphosphate, a polycarboxylate, and a polyether derivative.

[0007] According to an embodiment of the present invention, the solid content of the slurry is 30-60wt%; the particle size distribution of the phosphorus-carbon composite is 0.1-10 μm, and the mass content of phosphorus in the phosphorus-carbon composite is 20-80%.

[0008] According to an embodiment of the present invention, the Zeta potential of the aqueous phosphorus-carbon negative electrode slurry is maintained at -60~-40mV during a test time of 600 seconds.

[0009] According to an embodiment of the present invention, the added mass of the dispersant is 0.1-0.5% of the added mass of the water.

[0010] According to an embodiment of the present invention, the mass of the binder is 0.5~10% of the phosphorus-carbon composite, and the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, lithium polyacrylic acid, polyvinyl alcohol, chitosan, polytetrafluoroethylene, and polyvinylidene fluoride; the mass of the conductive agent is 0.5~10% of the phosphorus-carbon composite, and the conductive agent includes at least one of Ketjen black, acetylene black, conductive carbon black, graphene, carbon nanotubes, graphite, and hard carbon.

[0011] According to an embodiment of the present invention, the mass ratio of the binder to the conductive agent is 1:0.8 to 1:1.2.

[0012] According to an embodiment of another aspect of the present invention, there is provided a method for preparing an aqueous phosphorus-carbon negative electrode slurry as described above, comprising: sequentially adding a dispersant, a phosphorus-carbon composite, a conductive agent, and a binder into water, performing shear flow under the action of shear force, and obtaining an aqueous phosphorus-carbon negative electrode slurry.

[0013] According to an embodiment of the present invention, the surface of the phosphorus-carbon composite is pre-treated by oxidation before being added into water.

[0014] According to another embodiment of the present invention, there is provided a phosphorus-carbon negative electrode, which is prepared by the aqueous phosphorus-carbon negative electrode slurry as described above.

[0015] According to another embodiment of the present invention, there is provided a lithium-ion battery, comprising the phosphorus-carbon negative electrode as described above.

[0016] According to an embodiment of the present invention, by using a phosphorus-carbon composite as a negative electrode active material, phosphorus has a higher theoretical capacity, can provide additional lithium ion embedding sites, increase the lithium storage capacity of the negative electrode material, and the carbon material helps to improve the conductivity and structural stability of the composite. The addition of a binder helps to adhere the active material, conductive agent, etc. to the current collector, and after drying, it can promote the particles inside the negative electrode to effectively adhere together, which helps to ensure the mechanical strength and electrical contact of the negative electrode, thereby improving the adhesion of the negative electrode and the cycle stability of the lithium ion battery. The addition of a conductive agent helps to improve the electronic conductivity of the negative electrode, helps to quickly transmit lithium ions inside the negative electrode, and helps to improve the charge and discharge power and power density of the lithium ion battery. The present invention uses an aqueous slurry and cooperates with the above-mentioned ingredients to help disperse the phosphorus-carbon composite uniformly and stably in the water system and reduce the occurrence of flocculation. Compared with organic solvents, aqueous systems are more environmentally friendly, lower cost, and easy to handle, reducing environmental hazards. Adding the above-mentioned dispersant helps to reduce the aggregation of active materials, improve the rheological properties of the slurry, and improve the dispersibility and stability of the slurry. The solid content and viscosity of the slurry are controlled within the above ranges, and while the energy density of the subsequently prepared battery is increased, the viscosity of the slurry is ensured to be moderate, and good rheological properties are provided during the subsequent coating process to ensure uniform coating. The above-mentioned aqueous phosphorus-carbon negative electrode slurry formulation can be directly used for the coating of the pole piece of the phosphorus-carbon negative electrode, which can simplify the process and production costs. When the above-mentioned aqueous phosphorus-carbon negative electrode slurry formulation is used to prepare a phosphorus-carbon negative electrode and further assemble a lithium-ion battery, the battery test results show good rate capacity performance and cycle stability.

[0017] According to an embodiment of the present invention, by sequentially adding a phosphorus-carbon composite, a dispersant, a conductive agent, and a binder into water and using a liquid phase shear mixing method, a stably dispersed aqueous phosphorus-carbon negative electrode slurry system without coagulation can be obtained.

[0018] According to an embodiment of the present invention, the phosphorus-carbon composite requires a large amount of energy input during the preparation process, and the prepared phosphorus-carbon negative electrode material is prone to oxidation and may burn in severe cases. By introducing an aqueous slurrying process, the preparation of the phosphorus-carbon composite and the process of the aqueous phosphorus-carbon negative electrode slurry can be carried out continuously, and the water seal isolates oxygen to avoid oxidation or combustion of the phosphorus-carbon composite, which is conducive to achieving large-scale production and promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:

[0020] Figure 1 The scanning electron microscope image of the phosphorus carbon particles 1 after high pressure homogenization in Example 1 of the present invention is shown;

[0021] Figure 2 The scanning electron microscope image of the sand-polished phosphorus-carbon composite 1 of Example 1 of the present invention is shown;

[0022] Figure 3 The Zeta potential test curve of the aqueous phosphorus-carbon negative electrode slurry 1 before and after defoaming in Example 1 of the present invention is shown;

[0023] Figure 4 The charge / discharge curve diagram of the first three cycles of the phosphorus-carbon negative electrode battery 1 of Example 1 of the present invention is shown;

[0024] Figure 5 The graph showing the change of the charge / discharge specific capacity of the phosphorus-carbon negative electrode battery 1 according to Example 1 of the present invention with the number of cycles;

[0025] Figure 6 shows a scanning electron microscope image of negative electrode slurry 2 of Example 2 of the present invention;

[0026] Figure 7 The Zeta potential test curve of the aqueous phosphorus-carbon negative electrode slurry 2 before and after defoaming in Example 2 of the present invention is shown;

[0027] Figure 8 The charge / discharge curve diagram of the first three cycles of the phosphorus-carbon negative electrode battery 2 of Example 2 of the present invention is shown;

[0028] Fig. 9 The graph showing the change of the charge / discharge specific capacity of the phosphorus-carbon negative electrode battery 2 according to Example 2 of the present invention with the number of cycles;

[0029] Fig.10 The contact angle test results of the phosphorus-carbon negative electrode 2' in Comparative Example 2 of the present invention and the phosphorus-carbon negative electrode 2 in Example 2 to water are shown; and

[0030] Fig.11 The rate curves of the phosphorus-carbon negative electrodes prepared in Examples 1 and 2 of the present invention and Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0031] Below, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of embodiments of the present invention. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of concepts of the present invention.

[0032] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The term "comprising" used herein indicates the existence of features, steps, operations, but does not exclude the existence or addition of one or more other features.

[0033] In the case of using expressions such as "at least one of A, B, and C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.). In the case of using expressions such as "at least one of A, B, or C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, or C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).

[0034] In the present invention, the term "Zeta potential" refers to an important parameter that characterizes the surface charge state of the phosphorus-carbon composite particles in the aqueous phosphorus-carbon negative electrode slurry, and reflects the potential difference between the surface charge of the phosphorus-carbon composite particles and the surrounding slurry.

[0035] In the related technologies, there are few reports on the research of phosphorus-carbon negative electrode slurry, and phosphorus-carbon negative electrode is still in the exploratory stage.

[0036] In the process of realizing the concept of the present invention, it is found that by using a phosphorus-carbon composite as a negative electrode active material, the lithium storage capacity, conductivity and stability of the negative electrode material are improved. By using an aqueous slurry, that is, using water as the main solvent, and combining a binder, a conductive agent and a dispersant, it is helpful to achieve a uniform and stable dispersion of the phosphorus-carbon composite in the aqueous system, avoiding the coagulation phenomenon caused by the addition of the phosphorus-carbon composite to water. Controlling the solid content and viscosity of the slurry within a certain range can ensure the uniformity of the coating while increasing the energy density of the battery. And the above-mentioned aqueous phosphorus-carbon negative electrode slurry can be directly used for the coating of the pole piece of the phosphorus-carbon negative electrode, which helps to simplify the process and production costs.

[0037] Specifically, according to an embodiment of one aspect of the present invention, there is provided an aqueous phosphorus-carbon negative electrode slurry, comprising: a phosphorus-carbon composite, a binder, a conductive agent, water and a dispersant, wherein the phosphorus-carbon composite is an insoluble solid, and in the aqueous phosphorus-carbon negative electrode slurry, the slurry solid content is 10-70wt%, and the viscosity of the aqueous phosphorus-carbon negative electrode slurry ranges from 2000 to 12000mPa·s; the dispersant comprises at least one of polyphosphate, polycarboxylate and polyether derivative.

[0038] According to an embodiment of the present invention, the solid content of the slurry may be, for example, 20%, 30%, 40%, 50%, or 60%. Controlling the solid content of the slurry within the above range can determine the concentration of the active material (phosphorus-carbon complex) in the slurry. A high solid content can increase the energy density of the subsequently prepared lithium-ion battery, but if the solid content is too high, the viscosity of the slurry may increase, affecting the uniformity of the coating. The viscosity of the above-mentioned negative electrode slurry may be, for example, 3000mPa·s, 4000mPa·s, 5000mPa·s, 6000mPa·s, 7000mPa·s, 8000mPa·s, 9000mPa·s, 10000mPa·s or 11000mPa·s, but is not limited thereto. The viscosity range of the above-mentioned negative electrode slurry ensures that the slurry has good rheological properties during the coating process, and is neither too thin, resulting in uneven coating, nor too thick, resulting in difficulty in coating. The solid content and viscosity of the slurry are controlled within the above ranges, and the viscosity of the slurry is ensured to be moderate while the energy density of the subsequently prepared battery is increased, so that the slurry has good rheological properties in the subsequent coating process and the coating uniformity is ensured. The polyphosphate in the dispersant can improve the stability of the negative electrode slurry, reduce the aggregation of the particles of the phosphorus-carbon complex, and help to form a uniform phosphorus-carbon negative electrode in the subsequent process. The negative charge and higher molecular chain of the polycarboxylate help to stabilize the rheological properties of the negative electrode slurry, reduce the aggregation of the particles of the phosphorus-carbon complex, and improve the rheological properties of the negative electrode slurry. The surface activity and hydrophilicity of the polyether derivative help to improve the dispersibility and stability of the slurry.

[0039] According to an embodiment of the present invention, by using a phosphorus-carbon composite as a negative electrode active material, the phosphorus therein has a higher theoretical capacity, can provide additional lithium ion embedding sites, and increase the lithium storage capacity of the negative electrode material. The carbon material helps to improve the conductivity and structural stability of the composite. The use of a phosphorus-carbon composite helps to improve the theoretical capacity and lithium storage capacity of the phosphorus-carbon negative electrode, while also ensuring that it has good conductivity and cycle stability. The addition of a binder can promote the effective adhesion of particles inside the negative electrode after drying, help to adhere active materials, conductive agents, etc. to the current collector, and help to ensure the mechanical strength and electrical contact of the phosphorus-carbon negative electrode, thereby improving the adhesion of the negative electrode and the cycle stability of the lithium-ion battery. The addition of a conductive agent helps to improve the electronic conductivity of the negative electrode, helps to transmit lithium ions more quickly inside the negative electrode, and improves the charge and discharge power and power density of the lithium-ion battery. The present invention uses an aqueous slurry and is combined with the above-mentioned ingredients to help disperse the phosphorus-carbon composite uniformly and stably in the water system and reduce the occurrence of flocculation. Compared with organic solvents, aqueous systems are more environmentally friendly, have lower costs, and are easy to handle, reducing environmental hazards. The above-mentioned aqueous phosphorus-carbon negative electrode slurry can be directly used for the coating of the pole piece of the phosphorus-carbon negative electrode, thereby simplifying the process and production cost. When the phosphorus-carbon negative electrode is prepared using the above-mentioned aqueous phosphorus-carbon negative electrode slurry and further assembled into a lithium-ion battery, the battery test results show good rate capacity and cycle stability.

[0040] Preferably, the solid content of the slurry is 30-60 wt %. In the process of conducting relevant experiments of the present invention, it is found that when the solid content of the slurry is within the above range, the energy density of the prepared lithium ion battery is higher and the cycle stability is better.

[0041] According to an embodiment of the present invention, the particle size of the phosphorus-carbon composite is distributed in 0.1~10μm, for example, it can be 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm or 9μm, but it is not limited thereto. When the particle size of the phosphorus-carbon composite is within the above range, it helps to form a close contact between phosphorus and carbon, thereby forming an interaction force between the phosphorus-carbon interface, and when the particle size of the phosphorus-carbon composite is within the above range, it helps to improve its specific surface area and dispersion uniformity in an aqueous solvent, and reduce the occurrence of flocculation. The mass content of phosphorus in the phosphorus-carbon composite is 20~80%, for example, it can be 30%, 40%, 50%, 60% or 70%, but it is not limited thereto. Among them, the phosphorus in the phosphorus-carbon composite can be, for example, at least one of red phosphorus and black phosphorus, preferably red phosphorus. The carbon in the phosphorus-carbon composite can be, for example, at least one of graphite, hard carbon, conductive carbon, porous carbon, graphene, and carbon nanotubes, preferably graphite.

[0042] According to an embodiment of the present invention, the Zeta potential of the aqueous phosphorus-carbon negative electrode slurry can be maintained at -60~-40mV within a test time of 600 seconds, for example, it can be -55mV, -50mV or -45mV, but it is not limited thereto. The Zeta potential indicates the repulsive force between the particles of the phosphorus-carbon composite. Within the above potential range, the surface of the particles carries a strong negative charge, resulting in electrostatic repulsion between the particles, which helps to prevent particle aggregation and helps to maintain the uniformity and stability of the above negative electrode slurry. The above potential interval range also helps to control the rheological properties of the negative electrode slurry, helps to make the subsequent coating process smoother, and reduces defects such as holes and cracks during the coating process, thereby improving the consistency of the phosphorus-carbon negative electrode and the overall performance of the lithium-ion battery. Good uniformity and stability of the negative electrode slurry can improve the electrochemical reaction activity of the phosphorus-carbon negative electrode, and help to improve the charge and discharge efficiency and cycle stability of the lithium-ion battery.

[0043] According to an embodiment of the present invention, the added mass of the dispersant can be 0.1-0.5% of the added mass of water, for example, 0.2%, 0.3% or 0.4%. In the process of conducting relevant experiments of the present invention, it is found that when the dispersant is used in the above range, it is helpful to uniformly disperse the phosphorus-carbon complex in the aqueous phosphorus-carbon negative electrode slurry and avoid the coagulation phenomenon of the phosphorus-carbon complex in the aqueous phosphorus-carbon negative electrode slurry.

[0044] According to an embodiment of the present invention, the mass of the binder can be 0.5-10% of the phosphorus-carbon composite, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, but is not limited thereto. The binder may include at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, lithiated polyacrylic acid, polyvinyl alcohol, chitosan, polytetrafluoroethylene, and polyvinylidene fluoride, preferably chitosan or polyacrylic acid. When the mass of the binder is within the above range, the mechanical stability and electrochemical performance of the phosphorus-carbon negative electrode can be improved.

[0045] According to an embodiment of the present invention, the mass of the conductive agent can be 0.5-10% of the phosphorus-carbon composite, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, but is not limited thereto. The conductive agent can include at least one of Ketjen black, acetylene black, conductive carbon black, graphene, carbon nanotubes, graphite, and hard carbon, preferably one or more of graphite, graphene or carbon nanotubes. When the mass of the conductive agent is within the above range, it helps to improve the electronic conductivity of the phosphorus-carbon negative electrode and enhance the charge and discharge performance and energy density of the lithium-ion battery.

[0046] According to an embodiment of the present invention, the mass ratio of the binder to the conductive agent may be 1:(0.8-1.2), for example, 1:0.8, 1:0.9, 1:1, 1:1.1 or 1:1.2, but not limited thereto. By adjusting the binder and the conductive agent within the above range, a balance can be found between the mechanical strength and conductivity of the phosphorus-carbon negative electrode, so that the phosphorus-carbon negative electrode has both high conductivity and good bonding strength and overall stability, which helps to improve the charge and discharge efficiency, cycle stability and power density of the lithium-ion battery.

[0047] According to an embodiment of another aspect of the present invention, there is provided a method for preparing an aqueous phosphorus-carbon negative electrode slurry as described above, comprising: sequentially adding a dispersant, a phosphorus-carbon composite, a conductive agent, and a binder into water, performing shear flow under the action of shear force, and obtaining an aqueous phosphorus-carbon negative electrode slurry.

[0048] According to an embodiment of the present invention, a dispersion is formed by sequentially adding a dispersant, a phosphorus-carbon complex, a conductive agent, and a binder to water, and shear flow occurs inside the dispersion under the action of shear force to reduce the occurrence of coagulation. A uniform dispersion and mixing of an aqueous phosphorus-carbon negative electrode slurry is achieved. Shear flow can be achieved, for example, by using instruments such as an ultrasonic machine, a homogenizer, a sand mill, a ball mill, a high-speed mixer, or an ultrasonic cell crusher. Specifically, dissolving a dispersant in water first and then adding a phosphorus-carbon complex helps to improve the dispersibility of the phosphorus-carbon complex in water, reduce the agglomeration of the particles of the phosphorus-carbon complex, and form a stable phosphorus-carbon complex slurry and then adding a conductive agent to enable the conductive agent to be better dispersed between the particles of the phosphorus-carbon complex. Finally, adding a binder can disperse the binder molecules between the phosphorus-carbon complex and the conductive agent particles, and fiberize the binder molecules under the action of shear force, while increasing the viscosity of the entire aqueous phosphorus-carbon negative electrode slurry, which is beneficial to subsequent coating operations.

[0049] According to an embodiment of the present invention, after shear flow, the aqueous phosphorus-carbon negative electrode slurry can also be defoamed. Its function is to drive out the tiny bubbles in the water to prevent the bubbles from adhering to the surface of the particles of the phosphorus-carbon composite, thereby ensuring that the slurry can completely infiltrate the particles, conductive agent molecules and binder molecules of the phosphorus-carbon composite, and improve the stability of the negative electrode slurry system. And eliminating bubbles in the water helps to reduce the oxygen content, thereby inhibiting the oxidative degradation of phosphorus in water and improving the effective storage period of the negative electrode slurry.

[0050] According to an embodiment of the present invention, by introducing an aqueous slurrying process, the slurrying process is the entire preparation process from the phosphorus-carbon raw material or the phosphorus-carbon composite to the aqueous phosphorus-carbon negative electrode slurry, which helps to continuously carry out the preparation process of the phosphorus-carbon negative electrode material and the process of the aqueous phosphorus-carbon negative electrode slurry, and through the sealing and deoxygenation effect of water, the oxidation and even combustion of the phosphorus-carbon negative electrode is avoided, which is conducive to large-scale safe production. And the use of aqueous phosphorus-carbon negative electrode slurry can significantly reduce production costs and reduce environmental hazards compared to the use of oily slurry (using N-methylpyrrolidone as a dispersing solvent).

[0051] According to an embodiment of the present invention, the surface of the phosphorus-carbon composite may be subjected to oxidation pretreatment before being added to water. For example, water vapor is used to perform oxidation pretreatment on the phosphorus-carbon composite to introduce oxygen-containing groups, thereby achieving an etching effect, increasing the roughness of the surface of the particles of the phosphorus-carbon composite, and increasing the specific surface area of ​​the phosphorus-carbon composite, thereby helping to improve the wettability and dispersibility of the particles of the phosphorus-carbon composite to water, and reducing the amount of dispersant used.

[0052] According to an embodiment of the present invention, the oxidation pretreatment of the phosphorus-carbon compound may be an oxidation pretreatment of the phosphorus-carbon complex itself, or an oxidation pretreatment of the phosphorus element and the carbon-containing compound separately before forming the phosphorus-carbon complex.

[0053] According to an embodiment of the present invention, the conditions for the oxidation pretreatment may be: the heating temperature is 110-130° C., preferably 120° C. The heating time is 20-40 min, for example, 25 min, 30 min, 35 min, preferably 30 min, and water vapor is introduced into the reaction device while heating, and the flow rate of the water vapor is 80-120 sccm, for example, 90 sccm, 100 sccm, 110 sccm, but not limited thereto.

[0054] According to an embodiment of the present invention, a phosphorus-carbon composite can be obtained through the following preparation process: after mixing water and a metaphosphate dispersant, phosphorus element and a carbon-containing compound are added and stirred to obtain a dispersion; the dispersion is crushed and sheared to reduce the particle sizes of the phosphorus element and the carbon-containing compound therein to less than 5 μm, respectively, to form phosphorus-carbon particles; the crushed and sheared phosphorus-carbon particles are sand-milled and compounded to obtain a phosphorus-carbon composite.

[0055] According to the embodiment of the present invention, the particle size of the phosphorus element in the prepared phosphorus-carbon composite is reduced to submicron level, and the carbon-containing compound is sheared and broken into thin slices with a particle size of less than 5 μm.

[0056] According to an embodiment of the present invention, the phosphorus element may be, for example, red phosphorus or black phosphorus, preferably red phosphorus; the carbon-containing compound may be, for example, at least one of graphite and carbon nanotubes.

[0057] According to an embodiment of the present invention, the metaphosphate may be, for example, sodium hexametaphosphate, and the crushing shearing conditions are: homogenizing and crushing at a pressure of 1400-1600 bar, for example, 1500 bar, for a crushing time of 1-3 hours, for example, 2 hours, so that the particle sizes of the phosphorus element and the carbon-containing compound are reduced to less than 5 μm, respectively. The conditions for the sand milling and crushing compound are: using 0.2 mm zirconium beads at a speed of 3500-4500 rpm, for example, 4000 rpm, for circulating feeding grinding, and the grinding time is 10-14 hours, for example, 12 hours.

[0058] According to another embodiment of the present invention, there is provided a phosphorus-carbon negative electrode, which is prepared by the above-mentioned aqueous phosphorus-carbon negative electrode slurry.

[0059] According to an embodiment of the present invention, the aqueous phosphorus-carbon negative electrode slurry can be directly used for coating the pole piece of the phosphorus-carbon negative electrode, and the obtained phosphorus-carbon negative electrode exhibits excellent electrochemical properties in the lithium-ion battery system, with good capacity utilization, fast charging performance and good cycle stability.

[0060] According to another embodiment of the present invention, there is provided a lithium-ion battery comprising the phosphorus-carbon negative electrode as described above.

[0061] According to the embodiments of the present invention, the lithium-ion battery of the present invention has a higher energy density, a higher power density and better cycle stability, which is helpful for subsequent application in energy storage devices.

[0062] In a specific embodiment, a half-cell is assembled with lithium metal as the counter electrode, and the first discharge can provide a specific capacity of more than 1300mAh / g at a current density of 0.5A / g, and after 400 cycles, the specific capacity is still maintained at more than 1100mAh / g. And at a high current density of 6A / g (about 6-C), the specific capacity is still maintained at more than 800mAh / g.

[0063] The present invention is further described below by examples, drawings and related test experiments and results thereof. In the detailed description below, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present invention. However, it is obvious that one or more embodiments may also be implemented without these specific details. And, in the absence of conflict, the details in the following embodiments may be combined arbitrarily into other feasible embodiments.

[0064] It should be noted that the following specific examples are only for illustration, and the protection scope of the present invention is not limited thereto. The chemicals and raw materials used in the following examples are all commercially available or homemade by recognized processing methods.

[0065] Embodiment 1:

[0066] An aqueous phosphorus-carbon negative electrode slurry 1 is directly prepared starting from phosphorus and carbon raw materials, a phosphorus-carbon electrode 1 is further prepared, and a phosphorus-carbon negative electrode battery 1 is assembled.

[0067] Oxidation pretreatment of phosphorus and carbon surfaces:

[0068] Weigh 30g of red phosphorus and 30g of graphite powder, grind them in a mortar for 10 minutes for preliminary mixing, and then transfer the mixed powder into a quartz boat. Transfer the quartz boat to the center of the quartz tube of the tube furnace. The inner diameter of the quartz tube is 15cm and the length is 1.2m. Then seal both ends of the quartz tube and leave an air hole on each. Turn on the tube furnace for heating and set the temperature to 120℃. After the temperature stabilizes, pass water vapor into the quartz tube at a flow rate of 100±20sccm. Stop passing the gas after 30min. Turn off the tube furnace for heating after 5min, and take out the sample in the quartz tube.

[0069] Take 2L of deionized water, add 3g of sodium hexametaphosphate powder, and stir to dissolve in a large beaker. Transfer the steam-treated red phosphorus and graphite powders to a beaker, use a magnetic stirrer, and stir at 1000 rpm for 1 hour to mix the materials evenly to obtain a raw material dispersion.

[0070] The raw material dispersion was transferred to the feed tank of a high-pressure homogenizer (maximum processing capacity 12L / h), and the raw material dispersion was homogenized and crushed for 2 hours at a working pressure of 1500bar. Under the effects of cavitation effect, impact effect and shear effect, the particle size of red phosphorus and graphite in the raw material dispersion was reduced to less than 5μm, and phosphorus-carbon particles 1 after high-pressure homogenization were obtained. Figure 1 The scanning electron microscope image of the phosphorus-carbon particles 1 after high pressure homogenization in Example 1 of the present invention is shown. It can be seen that the red phosphorus and graphite have not yet formed a composite.

[0071] Preparation of phosphorus-carbon complex 1:

[0072] The phosphorus-carbon particles 1 treated by the high-pressure homogenizer were transferred to the feeding tank of the horizontal sand mill for sand milling and crushing. The effective volume of the sand mill grinding chamber was 0.6 L, 0.2 mm zirconium beads and stainless steel gaps with a spacing of 0.1 mm were used, and the feeding was circulated and ground for 12 hours at a speed of 4000 rpm. Figure 2 FIG. 2 shows a scanning electron microscope image of the sand-polished phosphorus-carbon composite 1 of Example 1 of the present invention. Figure 2 As shown, it can be seen that the red phosphorus and graphite raw materials have been effectively compounded after sand grinding, the particle size of red phosphorus is reduced to submicron level, the graphite is sheared and broken into thin flakes with a particle size of less than 5μm, and the red phosphorus is attached to the surface of the graphite particles.

[0073] Preparation of aqueous phosphorus-carbon negative electrode slurry 1:

[0074] The slurry of the phosphorus-carbon composite 1 in the sand mill was taken out, and most of the solvent was removed by vacuum filtration, and the volume of the remaining solid-liquid mixture was about 300 mL. The remaining solid-liquid mixture was transferred to the mixing tank of a high-speed mixer (VMA-GETZMANN mixer), and 2 g of Ketjen black powder was added at one time, and stirred and mixed at a speed of 10,000 rpm for 1 hour. Then 2 g of chitosan powder was added to the mixing tank, and the stirring and mixing was continued for 1 hour to completely dissolve the chitosan, and the sample was collected after the end.

[0075] The collected samples were transferred to a vacuum centrifugal degassing machine, and the degassing machine was turned on with a stirring speed of 2200 rpm for 15 minutes to fully mix the materials in the container and perform defoaming treatment. While stirring, the vacuum pump generates a vacuum environment in the container to remove the bubbles in the material. At this time, the aqueous phosphorus-carbon negative electrode slurry 1 is obtained. The viscosity of the tested slurry is 8200 mPa·s, which can be directly used for coating and preparing phosphorus-carbon negative electrode sheets. The Zeta potential of the slurry was tested before and after the defoaming treatment. Figure 3 The Zeta potential test curve of the aqueous phosphorus-carbon negative electrode slurry 1 before and after defoaming in Example 1 of the present invention is shown. Figure 3 As shown, it can be seen that the slurry stability is significantly improved after defoaming, and is maintained at around -45mV during the test time of 600 seconds.

[0076] Process for preparing the phosphorus-carbon negative electrode 1 using the aqueous phosphorus-carbon negative electrode slurry 1:

[0077] The obtained aqueous phosphorus-carbon negative electrode slurry 1 was coated and transferred to the surface of the copper foil current collector and vacuum dried at 80°C for 12 hours. After drying, it was naturally cooled in a drying oven and then taken out and cut into phosphorus-carbon negative electrodes 1 with a diameter of 10 mm. The active material surface loading was calculated to be 2.2 mg / cm 2 .

[0078] Testing process of the performance of phosphorus-carbon negative electrode 1:

[0079] A phosphorus-carbon negative electrode 1 was used as the working electrode, a metal lithium foil with a thickness of 300 μm was used as the counter electrode, 25 μL of electrolyte was added, the specific formula was 1 mol / L lithium hexafluorophosphate (LiPF6) dissolved in a solution of ethylene carbonate-diethyl carbonate (EC:DEC=1:1 volume ratio), a 21 μm thick polypropylene separator was used, and a CR2032 standard button cell was assembled, which was the phosphorus-carbon negative electrode battery 1.

[0080] For the phosphorus-carbon negative electrode battery 1, a long cycle test was carried out at a current density of 0.5 A / g, and the charge and discharge voltage range of the battery was 0.01~2.00V. Figure 4 The charge / discharge curve diagram of the first three cycles of the phosphorus-carbon negative electrode battery 1 of Example 1 of the present invention is shown. Figure 5 The graph showing the change of the charge / discharge specific capacity of the phosphorus-carbon negative electrode battery 1 according to Example 1 of the present invention with the number of cycles is shown. Figure 4 and Figure 5 As shown, at a current density of 0.5A / g, the first cycle discharge capacity of the phosphorus-carbon negative electrode battery 1 is 1347mAh / g, and it still maintains a capacity of 1018mAh / g at the 400th cycle. The rate performance test was carried out at current densities of 0.5A / g, 1.0A / g, 2.0A / g, 4.0A / g, and 6.0A / g, and the average discharge capacity at different rate currents was recorded. The specific data is shown in Table 1 below.

[0081] Embodiment 2:

[0082] The pre-synthesized phosphorus-carbon composite 2 is used to prepare an aqueous phosphorus-carbon negative electrode slurry 2, and a phosphorus-carbon electrode 2 is further prepared to assemble a phosphorus-carbon negative electrode battery 2.

[0083] Preparation of phosphorus-carbon complex 2:

[0084] 20g of phosphorus-carbon composite powder prepared by high-energy ball milling process contains 50% red phosphorus, 40% graphite and 10% carbon nanotubes by mass. According to the same oxidation pretreatment method as in Example 1, the phosphorus-carbon composite powder is treated with water vapor in a tube furnace for 30 minutes, and the sample is taken out.

[0085] Preparation of aqueous phosphorus-carbon negative electrode slurry 2:

[0086] Take a 50mL glass beaker, add 40mL deionized water and 0.2g polycarboxylate dispersant, place the beaker on a magnetic stirrer, add a magnet, start stirring at 500rpm. After stirring for 10 minutes, transfer all the phosphorus-carbon composite powder to the beaker. Continue stirring and mixing for 1h, then add 0.8g of graphene powder to the beaker, increase the speed to 1200rpm, and continue stirring and mixing for 1h.

[0087] Add 0.8 g of water-soluble polyacrylic acid (PAA) binder (powder, average molecular weight about 450,000) to the beaker and continue stirring at 1200 rpm for 1 hour. After PAA is completely dissolved and evenly dispersed, transfer the slurry into a 50 mL centrifuge tube and continue to process for 1 hour using an ultrasonic cell crusher. The equipment operates at 500 W, the horn is immersed in the water to a depth of about 1.5 cm, and the probe is centered. After the treatment, the solid particles in the slurry were characterized by scanning electron microscopy. Figure 6 FIG. 2 shows a scanning electron microscope image of the aqueous phosphorus-carbon negative electrode slurry 2 of Example 2 of the present invention. Figure 6As shown, it can be seen that the fiberized binder is attached to the surface of the solid particles, playing a good cross-linking role, increasing the viscosity of the aqueous phosphorus-carbon negative electrode slurry 2, and facilitating the subsequent coating operation.

[0088] The treated aqueous phosphorus-carbon negative electrode slurry 2 was transferred to the container of the vacuum centrifugal degassing machine, and the container was kept in a near vacuum environment. The degassing machine stirred at a speed of 2200rpm and worked for 10 minutes to fully mix the materials in the container and remove the bubbles in the materials. At this time, the defoamed aqueous phosphorus-carbon negative electrode slurry 2 was obtained, and the viscosity of the tested slurry was 6000mPa·s. The Zeta potential of the slurry was tested before and after the defoaming treatment. Figure 7 The Zeta potential test curve of the aqueous phosphorus-carbon negative electrode slurry 2 before and after defoaming in Example 2 of the present invention is shown. Figure 7 As shown, it can be seen that the stability of the aqueous phosphorus-carbon negative electrode slurry 2 is significantly improved after defoaming, and is maintained at around -40 mV during the test time of 600 seconds.

[0089] Process for preparing phosphorus-carbon negative electrode 2 using aqueous phosphorus-carbon negative electrode slurry 2:

[0090] According to the steps in Example 1, the aqueous phosphorus-carbon negative electrode slurry 2 was coated and transferred to the surface of the copper foil current collector. After drying, it was cut to prepare a phosphorus-carbon negative electrode 2 with a diameter of 10 mm. The active material surface loading was calculated to be 2.1 mg / cm 2 .

[0091] Testing process of the performance of phosphorus-carbon negative electrode 2:

[0092] According to the battery assembly and testing method in Example 1, the phosphorus-carbon negative electrode 2 was used as the working electrode to assemble the phosphorus-carbon negative electrode battery 2. The long cycle performance at a current density of 0.5 A / g and the rate performance at current densities of 0.5 A / g, 1.0 A / g, 2.0 A / g, 4.0 A / g, and 6.0 A / g were tested. The specific data are shown in Table 1 below. Figure 8 The charge / discharge curve diagram of the first three cycles of the phosphorus-carbon negative electrode battery 2 of Example 2 of the present invention is shown. Fig. 9 The graph showing the change of the charge / discharge specific capacity of the phosphorus-carbon negative electrode battery 2 according to Example 2 of the present invention with the number of cycles is shown. The results show that at a current density of 0.5 A / g, the first cycle discharge specific capacity of the phosphorus-carbon negative electrode 2 is 1233 mAh / g, and at the 400th cycle, the capacity is still 933 mAh / g.

[0093] Comparative Example 1:

[0094] In this comparative example 1, the pre-synthesized phosphorus-carbon composite 1' is directly coated with an oil system to prepare an electrode, and then a battery is assembled for testing.

[0095] Take 90 mg of the phosphorus-carbon composite powder 2 used in Example 2, mix it with a conductive agent (Ketjen black) and a binder (1 mg of polyvinylidene fluoride / 30 μL of N-methylpyrrolidone) in a mass ratio of 90:5:5, and use N-methylpyrrolidone (NMP) as a solvent to prepare the slurry. The prepared oil-based slurry 1' is coated on a copper current collector, and after vacuum drying at 80°C for 12 hours, a phosphorus-carbon negative electrode 1' is obtained, which is cut into electrode sheets with a diameter of 10 mm, and the active material surface loading is calculated to be 1.6 mg / cm 2 .

[0096] According to the battery assembly method in Example 1, the phosphorus-carbon negative electrode 1' in the previous step is used as the working electrode to assemble the phosphorus-carbon negative electrode battery 1'. The rate performance at current densities of 0.5A / g, 1.0A / g, 2.0A / g, 4.0A / g, and 6.0A / g is tested, and the specific data are shown in Table 1 below.

[0097] Comparative Example 2:

[0098] Comparative Example 2 is a control group using the pre-synthesized phosphorus-carbon composite 2' without performing a water vapor oxidation etching treatment.

[0099] According to the method in Example 2, the step of subjecting the phosphorus-carbon composite to water vapor oxidation etching was omitted, and the other conditions remained unchanged to prepare a phosphorus-carbon negative electrode 2' with a diameter of 10 mm. The active material surface loading was calculated to be 1.8 mg / cm 2 .

[0100] The contact angle test was performed on the phosphorus-carbon negative electrode 2' and the electrode obtained in Example 2 to measure the contact angles of water with the surfaces of the two electrode sheets. Fig.10 The contact angle test results of the phosphorus-carbon negative electrode 2' in Comparative Example 2 of the present invention and the phosphorus-carbon negative electrode 2 in Example 2 to water are shown. Fig.10 As shown, it can be seen that the contact angle before water vapor oxidation pretreatment is 43°, and the contact angle after water vapor oxidation pretreatment is 18°, indicating that water vapor oxidation increases the roughness of the surface of the phosphorus-carbon negative electrode, which significantly improves the wettability of the phosphorus-carbon negative electrode to water.

[0101] According to the battery assembly method in Example 1, the rate performance of the half-cell at current densities of 0.5 A / g, 1.0 A / g, 2.0 A / g, 4.0 A / g, and 6.0 A / g was tested. The specific data are shown in Table 1 below.

[0102] The average specific discharge capacities (unit: mAh / g) at different rates (current densities) obtained in Example 1, Example 2, Comparative Example 1, and Comparative Example 2 are summarized in Table 1 for comparison.

[0103] Table 1 Discharge specific capacity of Examples 1-2 and Comparative Examples 1-2 (unit: mAh / g)

[0104]

[0105] The above data can be organized into a point-line graph, such as Fig.11 As shown. The results show that the aqueous coated phosphorus-carbon negative electrode in Example 1 and Example 2 exhibits good rate performance, and has a better discharge specific capacity than the phosphorus-carbon negative electrode prepared by oily coating in Comparative Example 1 at a rate of 0.5A / g. At high rates of 1.0A / g and above, the specific capacity of the aqueous coated phosphorus-carbon negative electrode is significantly better than that of the oily prepared negative electrode sheet. In Comparative Example 2, although aqueous coating was also used, the phosphorus-carbon composite was not pretreated with steam oxidation (etching the surface), and its wettability with water was poor, and the performance of the obtained phosphorus-carbon negative electrode was significantly lower than that of Example 1 and Example 2. This is mainly attributed to the improved wettability and dispersibility of the pretreated phosphorus-carbon composite in water, and the aqueous phosphorus-carbon negative electrode slurry can better mix the phosphorus-carbon composite, conductive agent, binder and other components, so that the internal components of the above slurry and the phosphorus-carbon negative electrode obtained by coating and drying are uniform, the system is more stable, and the polarization caused by large current can be suppressed, thereby showing better rate performance.

[0106] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An aqueous phosphorus-carbon negative electrode slurry, comprising: A phosphorus-carbon composite, a binder, a conductive agent, water and a dispersant, wherein the phosphorus-carbon composite is an insoluble solid, the aqueous phosphorus-carbon negative electrode slurry has a solid content of 10-70wt%, and a viscosity range of 2000-12000mPa·s; The dispersant includes at least one of polyphosphate, polycarboxylate and polyether derivative.

2. The aqueous phosphorus-carbon negative electrode slurry according to claim 1, wherein The solid content of the slurry is 30-60wt%; the particle size distribution of the phosphorus-carbon composite is 0.1-10 μm, and the mass content of phosphorus in the phosphorus-carbon composite is 20-80%.

3. The aqueous phosphorus-carbon negative electrode slurry according to claim 1, wherein: The Zeta potential of the aqueous phosphorus-carbon negative electrode slurry was maintained at -60~-40mV during the test time of 600 seconds.

4. The aqueous phosphorus-carbon negative electrode slurry according to claim 1, wherein: The added mass of the dispersant is 0.1-0.5% of the added mass of water.

5. The aqueous phosphorus-carbon negative electrode slurry according to claim 1, wherein: The mass of the binder is 0.5-10% of the phosphorus-carbon composite, and the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, lithiated polyacrylic acid, polyvinyl alcohol, chitosan, polytetrafluoroethylene, and polyvinylidene fluoride; The mass of the conductive agent is 0.5-10% of the phosphorus-carbon composite, and the conductive agent includes at least one of Ketjen black, acetylene black, conductive carbon black, graphene, carbon nanotubes, graphite, and hard carbon.

6. The aqueous phosphorus-carbon negative electrode slurry according to claim 1, wherein: The mass ratio of the binder to the conductive agent is 1:0.8 to 1:1.

2.

7. A method for preparing an aqueous phosphorus-carbon negative electrode slurry as claimed in any one of claims 1 to 6, comprising: A dispersant, a phosphorus-carbon composite, a conductive agent and a binder are sequentially added to water, and shear flow is performed under the action of shear force to obtain the aqueous phosphorus-carbon negative electrode slurry.

8. The preparation method according to claim 7, wherein: Before being added into water, the surface of the phosphorus-carbon composite is subjected to oxidation pretreatment.

9. A phosphorus-carbon negative electrode prepared by the aqueous phosphorus-carbon negative electrode slurry according to any one of claims 1 to 6.

10. A lithium ion battery comprising the phosphorus-carbon negative electrode as claimed in claim 9.

Citation Information

Cited By

  • Negative plate, preparation method thereof and lithium ion secondary battery

    CN119993987A

  • Phosphorus-carbon negative electrode plate and preparation method thereof, sodium-ion battery and electric equipment

    CN120674431A

  • Phosphorus-carbon negative electrode aqueous slurry and preparation method thereof

    CN122025643A

  • A phosphorus-carbon anode aqueous slurry and its preparation method

    CN122025643B