Multifunctional passive film for modifying lithium anode and preparation method of multifunctional passive film

By using MgF2-PVDF-HFP passivation film in all-solid-state lithium batteries to generate a LiF/Mg-rich modified layer on the surface of the lithium anode, the problem of insufficient rigidity of the inorganic interlayer is solved, and uniform deposition and dendrite suppression of the lithium anode are achieved. , improves the cycle life and safety of the battery, and is suitable for industrial production.

CN118738286APending Publication Date: 2024-10-01GUIZHOU ZHONGSHUI MATERIAL TECH CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410904456.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In all-solid-state lithium batteries, the inorganic interlayer between the lithium anode and the solid electrolyte is insufficiently rigid and cannot withstand the volume change of the lithium anode, causing the interlayer to break and fall off. The preparation process is complex, which affects battery performance and safety.

Method used

Using MgF2-PVDF-HFP passivation film, a LiF/Mg-rich modification layer is generated by hot pressing on the lithium anode surface to enhance interface compatibility and adjust lithium deposition behavior, combined with high mechanical strength MgF2-PVDF-HFP passivation film and LiF/Mg modified layer to form a multifunctional passivation film to cope with volume changes and dendrite growth of lithium anodes.

Benefits of technology

It achieves uniform deposition of lithium anode during the electroplating/stripping process, inhibits dendrite growth, enhances the interface stability between lithium anode and electrolyte, improves the cycle life and safety of the battery, and has a simple process, low cost, and is suitable for industrial production. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738286A_ABST
    Figure CN118738286A_ABST
Patent Text Reader

Abstract

The invention discloses a multifunctional passivation film for modifying a lithium anode and a preparation method thereof, the material comprises the lithium anode and an MgF2-PVDF-HFP passivation film hot-pressed on the surface of the lithium anode, the MgF2-PVDF-HFP passivation film comprises MgF2 and PVDF-HFP, and in the hot pressing process, MgF2 and PVDF-HFP in the MgF2-PVDF-HFP passivation film and lithium in the lithium anode trigger an in-situ reaction to generate a modification layer rich in LiF / Mg. According to the multifunctional passivation film for modifying the lithium anode and the preparation method of the multifunctional passivation film, the magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene multifunctional passivation film is prepared by adopting a phase inversion method, and the inorganic filler MgF2 can effectively adjust the aperture and crystallinity of the passivation film; the LiF / Mg modified layer and the MgF2-PVDF-HFP middle passivation layer are in contact with each other to generate an in-situ reaction with PVDF-HFP passivator molecules and a lithium anode to generate a multifunctional passivation layer rich in LiF / Mg, so that the uniform deposition behavior of lithium in the electroplating / stripping process is adjusted, the formation of dendritic crystals is inhibited, and under the synergistic effect of the LiF / Mg modified layer and the MgF2-PVDF-HFP middle passivation layer, the interfacial compatibility between electrolyte and the lithium anode is effectively enhanced, and the performance of the electrolyte is improved. Therefore, highly reversible circulation is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of all-solid-state lithium battery materials, and in particular to a multifunctional passivation film for modifying a lithium anode and a preparation method thereof. Background Art

[0002] Lithium-ion batteries (LIBs) have been widely used in portable electronic devices, new energy vehicles, and energy storage systems. However, the low energy density of commercial LIBs can no longer meet people's needs. In addition, the liquid electrolytes used have safety hazards such as combustion and are prone to thermal runaway, which restricts their further development. Replacing flammable organic liquid electrolytes with solid electrolytes can meet high safety requirements. Lithium metal benefits from its ultra-high theoretical specific capacity (3860mAhg -1 ) and a low redox overpotential (-3.04 V), is considered to be an ideal "holy grail" anode material.

[0003] Based on this, all-solid-state batteries (ASSLBs) with lithium metal as anode have great potential in terms of high safety, energy density and power density. However, the interface between the lithium anode and the solid electrolyte is incompatible, and the presence of parasitic reactions and uneven lithium deposition will induce the wild growth of lithium dendrites and even pierce the electrolyte layer, resulting in capacity loss, unsatisfactory coulombic efficiency, short cycle life, safety hazards and battery failure.

[0004] To address these problems, constructing an intermediate artificial interface layer (LiF, Li3N, etc.) with high interfacial energy between the solid electrolyte and the lithium anode can effectively inhibit the growth of lithium dendrites and achieve uniform deposition of lithium during the electroplating / stripping process. However, the inorganic intermediate layer is too rigid to withstand the volume change of the lithium anode during the electroplating / stripping process, resulting in the intermediate layer breaking and falling off, causing battery failure, and the preparation process is complicated. The key to solving the above problems is to develop an electrolyte / lithium anode intermediate layer membrane material with excellent performance. Summary of the invention

[0005] The purpose of the present invention is to provide a multifunctional passivation film for modifying a lithium anode and a preparation method thereof, so as to solve the problem that the inorganic intermediate layer between the above-mentioned solid electrolyte and the lithium anode is too rigid and cannot withstand the volume change of the lithium anode during the electroplating / stripping process, resulting in the intermediate layer rupturing and falling off, causing battery failure, and the preparation process is complicated.

[0006] To achieve the above-mentioned purpose, the first aspect of the present invention provides a multifunctional passivation film for modifying a lithium anode, comprising a lithium anode and a MgF2-PVDF-HFP passivation film hot-pressed on the surface of the lithium anode, the MgF2-PVDF-HFP passivation film comprising MgF2 and PVDF-HFP, and during the hot-pressing process, the MgF2 and PVDF-HFP in the MgF2-PVDF-HFP passivation film trigger an in-situ reaction with the lithium in the lithium anode to generate a modified layer rich in LiF / Mg.

[0007] At present, the existing technology for setting an inorganic intermediate layer between a solid electrolyte and a lithium anode mostly adopts the method of directly preparing magnesium fluoride on the surface of the lithium anode. However, this direct preparation method cannot withstand the volume change caused by the lithium anode during the electroplating / stripping process, and the inorganic intermediate layer breaks and falls off, causing the battery to fail. In the present invention, magnesium fluoride is first doped into the passivation film, and the passivation film has good mechanical properties and elasticity, and can withstand the volume change caused by the lithium anode. At the same time, the inorganic filler magnesium fluoride can also adjust the pore size and crystallinity of the passivation film, thereby realizing the preparation of a multifunctional passivation film with a porous structure.

[0008] On the other hand, during the hot pressing of the passivation film onto the lithium anode, the multifunctionality of the MgF2-PVDF-HFP passivation film is mainly reflected in the following aspects:

[0009] (1) The MgF2 and PVDF-HFP passivation agent molecules in the passivation film trigger an in-situ reaction with lithium to generate a modified layer rich in LiF / Mg, thereby regulating the uniform deposition behavior of lithium during the electroplating / stripping process and inhibiting the formation of dendrites. This in-situ generation method greatly increases the interfacial compatibility between magnesium fluoride and the lithium anode, solves the problem of damage to the inorganic intermediate layer caused by the volume change of the lithium anode in the prior art, and reduces the shedding and cracking of the inorganic intermediate layer.

[0010] (2) The MgF2-PVDF-HFP passivation film also has the effect of hindering electron transfer and limiting the formation of dendrites within the layer. Even if some lithium dendrites grow unexpectedly and break through the LiF / Mg layer, they will be directly eliminated by the excess MgF2 in the MgF2-PVDF-HFP interlayer.

[0011] (3) The synergistic effect of the high mechanical strength MgF2-PVDF-HFP passivation layer and the high interfacial energy and high interfacial adhesion energy LiF / Mg modification layer effectively enhances the interfacial compatibility between the electrolyte and the lithium anode, thereby achieving highly reversible cycling. The lithium anode modified with this passivation film exhibits considerable electrochemical properties and is considered to be an ideal all-solid-state lithium battery material.

[0012] The second aspect of the present invention provides a method for preparing a multifunctional passivation film for modifying a lithium anode, comprising the following steps:

[0013] (1) Preparation of MgF2-PVDF-HFP passivation film precursor

[0014] Dissolve PVDF-HFP and MgF2 in acetone in turn, heat and stir, and after PVDF-HFP and MgF2 are completely dissolved, a uniform solution is obtained, deionized water is added to the uniform solution, and stirring is continued. After standing, a MgF2-PVDF-HFP passivation film precursor is obtained;

[0015] (2) Preparation of MgF2-PVDF-HFP passivation film

[0016] The viscous MgF2-PVDF-HFP passivation film precursor is evenly spread in a polytetrafluoroethylene mold using a scraper, and most of the acetone is volatilized at room temperature, and then treated in a vacuum drying oven to remove free solvent molecules to obtain a magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film, namely, a MgF2-PVDF-HFP passivation film;

[0017] (3) Construction of LiF / Mg-rich passivation layer on the lithium anode surface

[0018] The prepared MgF2-PVDF-HFP passivation film was hot pressed onto the surface of the lithium anode using a thermal driving method. After pressure treatment, a lithium anode modified with MgF2-PVDF-HFP was obtained, namely MgF2-PVDF-HFP@Li.

[0019] Preferably, the PVDF-HFP and MgF2 in step (1) are reagents that have been heated in vacuum to remove moisture.

[0020] Preferably, the specific process of heating and stirring in step (1) is: magnetic stirring for 10-12 hours at a rotation speed of 400-600 r / min and 50° C.; the stirring time is continued for 1-2 hours; and the standing time is 5-10 minutes.

[0021] Preferably, in step (1), the total mass of PVDF-HFP and MgF2 dissolved in every 10 mL of acetone is 1 g, wherein the mass ratio of PVDF-HFP to MgF2 is (96-100):(0-4).

[0022] Preferably, the volume ratio of the added amount of deionized water and acetone in step (1) is 1:(8-10).

[0023] Preferably, in step (2), the temperature of the vacuum drying oven is 60 to 80° C., and the treatment time is 24 to 48 hours.

[0024] Preferably, in step (3), the temperature of hot pressing is 70-90° C., the pressure is 0.8-1.4T, and the time of hot pressing is 1-2 hours.

[0025] Preferably, all operations in step (3) are performed in a glove box filled with an inert atmosphere.

[0026] Another key point of the present invention is the amount of PVDF-HFP and MgF2, the temperature, pressure and time of hot pressing, etc. The mass ratio of MgF2 to the total mass of MgF2 and PVDF-HFP is in the range of 0%-4%, the temperature of hot pressing is 70-90°C, the pressure of hot pressing is 0.8-1.4T, and the time of hot pressing is 1-2h. Only within this parameter range can the present invention prepare a multifunctional passivation film MgF2-PVDF-HFP with a porous structure, and the passivation film can be used to construct a LiF / Mg-rich artificial modified layer on the surface of the lithium anode.

[0027] Therefore, the present invention adopts a multifunctional passivation film for modifying a lithium anode and a preparation method thereof using the above structure, which has the following beneficial effects:

[0028] (1) The present invention utilizes a phase inversion method to prepare a MgF2-PVDF-HFP multifunctional passivation film with a uniform porous structure, which has the advantages of low cost, simple process, environmental friendliness, and can achieve large-scale industrial production.

[0029] (2) The present invention utilizes the MgF2-PVDF-HFP multifunctional passivation film to construct an artificial modified layer rich in LiF / Mg on the surface of the lithium anode, which can enhance the interfacial stability between the lithium anode and the electrolyte. In addition, LiF / Mg can induce uniform lithium deposition. On the other hand, LiF / Mg acts as a rivet to tightly connect the MgF2-PVDF-HFP film and Li, which is beneficial to maintaining the structural stability of the modified layer and ensuring the rapid transfer of lithium ions on the interface. The high mechanical strength MgF2-PVDF-HFP passivation film also has the effect of hindering electron transfer and can limit the formation of dendrites in the layer. Even if some accidentally grown Li dendrites break through the LiF / Mg layer, they will be directly eliminated by the excess MgF2 in the MgF2-PVDF-HFP interlayer. Therefore, under the synergistic effect of the high interfacial energy inorganic LiF / Mg modified layer and the high mechanical strength MgF2-PVDF-HFP intermediate passivation layer, the growth of lithium dendrites can be well suppressed, ensuring that they will not pierce the electrolyte layer, thereby improving the service life of the battery.

[0030] (3) The present invention utilizes MgF2-PVDF-HFP multifunctional passivation film to modify the lithium anode, which has the characteristics of simple operation, low cost, and can be industrialized.

[0031] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1The preparation flow chart of MgF2-PVDF-HFP@Li;

[0033] Figure 2 This is a digital photo of the MgF2-PVDF-HFP passivation film;

[0034] Figure 3 is a scanning electron microscope image of MgF2-PVDF-HFP;

[0035] Figure 4 X-ray diffraction patterns of PVDF-HFP and x%MgF2-PVDF-HFP (x=0.2, 0.3, 0.4) passivation films;

[0036] Figure 5 The scanning electron microscope (SEM) and corresponding mapping image of lithium anode modified with 3% MgF2-PVDF-HFP passivation film;

[0037] Figure 6 This is a test diagram of the critical current density of different lithium anodes;

[0038] Figure 7 At 0.1 mA cm -2 Constant current cycling curves of untreated Li and 3%MgF2-PVDF-HFP@Li symmetric cells at different current densities. DETAILED DESCRIPTION

[0039] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.

[0040] Example 1

[0041] A method for preparing a 2%MgF2-PVDF-HFP@Li symmetrical battery comprises the following steps:

[0042] Step 1, prepare 2% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film precursor: dissolve the PVDF-HFP and MgF2 from which the water has been removed in acetone in turn, wherein the total amount of PVDF-HFP and MgF2 dissolved in every 10 ml of acetone is 1 g, the total mass of the added PVDF-HFP and MgF2 is 100 equal parts, and the mass proportion of MgF2 is 2 equal parts. At a speed of 500 r / min and 50°C, magnetic stirring is performed for 12 hours. After PVDF-HFP and MgF2 are completely dissolved, 2 equal parts of deionized water are added to the uniform solution, stirring is continued for 1.5 hours, and after standing for 8 minutes, a 2% MgF2-PVDF-HFP passivation film precursor is obtained.

[0043] Step 2: Preparation of 2% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film: Use a scraper to evenly spread the above-obtained viscous 2% MgF2-PVDF-HFP passivation film precursor in a polytetrafluoroethylene mold. After most of the acetone is volatilized at room temperature, vacuum dry at 70°C for 36 hours to remove free solvent molecules to obtain a 2% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film, marked as 2% MgF2-PVDF-HFP.

[0044] Step 3: Constructing a LiF / Mg-rich modified layer on the surface of the lithium anode: Using a thermal drive method, the prepared passivation film 2% MgF2-PVDF-HFP was hot pressed onto the surface of the lithium anode at 80°C and treated at a pressure of 1.0 T for 1.5 hours. The lithium anode modified with 2% MgF2-PVDF-HFP was obtained, marked as 2% MgF2-PVDF-HFP@Li.

[0045] Step 4: First, 100 mg of Li6PS5Cl sulfide solid electrolyte powder was placed into a PEEK mold (diameter: 10 mm), and pressurized at a pressure of 1.4 T for 6 minutes to obtain a solid electrolyte layer.

[0046] Step 5: Place the lithium anode (diameter: 9 mm) processed in step 3 on both sides of the electrolyte layer prepared in step 4, and pressurize at 0.5T and maintain the pressure for 5 minutes. Finally, apply a constant pressure of 1T to the outer shell of the pressure mold to assemble a lithium-lithium symmetric battery, marked as 2%MgF2-PVDF-HFP@Li symmetric battery.

[0047] Example 2

[0048] A method for preparing a 3%MgF2-PVDF-HFP@Li symmetrical battery comprises the following steps:

[0049] Step 1, preparation of 3% magnesium fluoride-polytetrafluoroethylene-hexafluoropropylene passivation film precursor: dissolve the dehydrated PVDF-HFP and MgF2 in acetone in turn, wherein the total amount of PVDF-HFP and MgF2 dissolved in each 10ml of acetone is 1g, the total mass of PVDF-HFP and MgF2 added is 100 equal parts, and the mass proportion of MgF2 is 3 equal parts. Stir magnetically for 10 hours at a speed of 500r / min and 50°C. After PVDF-HFP and MgF2 are completely dissolved, add 2 equal parts of deionized water to the uniform solution and continue stirring for 1.5 hours. After standing for 8 minutes, a 3% MgF2-PVDF-HFP passivation film precursor is obtained.

[0050] Step 2: Preparation of 3% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film: Use a scraper to evenly spread the above-obtained viscous 3% MgF2-PVDF-HFP passivation film precursor in a polytetrafluoroethylene mold. After most of the acetone is volatilized at room temperature, vacuum dry at 70°C for 36 hours to remove free solvent molecules to obtain a 3% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film, marked as 3% MgF2-PVDF-HFP.

[0051] Step 3: Construct a LiF / Mg-rich modified layer on the surface of the lithium anode: Use a thermally driven method to hot-press the prepared passivation film 3% MgF2-PVDF-HFP onto the surface of the lithium anode at 80°C and treat it at a pressure of 1.0 T for 1.5 h to obtain a lithium anode modified with 3% MgF2-PVDF-HFP, labeled as 3% MgF2-PVDF-HFP@Li.

[0052] Step 4: First, 100 mg of Li6PS5Cl sulfide solid electrolyte powder was placed into a PEEK mold (diameter: 10 mm), and pressurized at a pressure of 1.4 T for 6 minutes to obtain a solid electrolyte layer.

[0053] Step 5: Place the lithium anode (diameter: 9 mm) processed in step 3 on both sides of the electrolyte layer prepared in step 4, and pressurize at 0.5T and maintain the pressure for 5 minutes. Finally, apply a constant pressure of 1T to the outer shell of the pressure mold to assemble a lithium-lithium symmetric battery, marked as 3%MgF2-PVDF-HFP@Li symmetric battery.

[0054] Example 3

[0055] A method for preparing a 4%MgF2-PVDF-HFP@Li symmetrical battery comprises the following steps:

[0056] Step 1. Prepare 4% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film precursor: dissolve the dehydrated PVDF-HFP and MgF2 in acetone in turn, wherein the total amount of PVDF-HFP and MgF2 dissolved in every 10 ml of acetone is 1 g, the total mass of PVDF-HFP and MgF2 added is 100 equal parts, and the mass proportion of MgF2 is 4 equal parts. Stir magnetically at a speed of 500 r / min and 50°C for 10 hours. After PVDF-HFP and MgF2 are completely dissolved, add 2 equal parts of deionized water to the uniform solution and continue stirring for 1.5 hours. After standing for 8 minutes, a 4% MgF2-PVDF-HFP passivation film precursor is obtained.

[0057] Step 2: Preparation of 4% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film: Use a scraper to evenly spread the above-obtained viscous 4% MgF2-PVDF-HFP passivation film precursor in a polytetrafluoroethylene mold. After most of the acetone is volatilized at room temperature, vacuum dry at 70°C for 36 hours to remove free solvent molecules to obtain a 4% magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film, marked as 4% MgF2-PVDF-HFP.

[0058] Step 3: Constructing a LiF / Mg-rich modified layer on the surface of the lithium anode: Using a thermal drive method, the prepared passivation film 4% MgF2-PVDF-HFP was hot pressed onto the surface of the lithium anode at 80°C and treated at a pressure of 1.0 T for 1.5 hours. The lithium anode modified with 4% MgF2-PVDF-HFP was obtained, marked as 4% MgF2-PVDF-HFP@Li.

[0059] Step 4: First, 100 mg of Li6PS5Cl sulfide solid electrolyte powder was placed into a PEEK mold (diameter: 10 mm), and pressurized at a pressure of 1.4 T for 6 minutes to obtain a solid electrolyte layer.

[0060] Step 5. Place the lithium anode (diameter: 9 mm) processed in step 3 on both sides of the electrolyte layer prepared in step 4, and pressurize at 0.5T and maintain the pressure for 5 minutes. Finally, apply a constant pressure of 1T to the outer shell of the pressure mold to assemble a lithium-lithium symmetric battery, marked as 4%MgF2-PVDF-HFP@Li symmetric battery.

[0061] Comparative Example 1

[0062] A method for preparing a PVDF-HFP@Li symmetrical battery comprises the following steps:

[0063] Step 1, preparation of polytetrafluoroethylene-hexafluoropropylene passivation film precursor: dissolve the dehydrated PVDF-HFP in acetone, wherein the total amount of PVDF-HFP dissolved in every 10 ml of acetone is 1 g. Stir magnetically for 10 hours at a speed of 500 r / min and 50°C. After the PVDF-HFP is completely dissolved (100 equal parts), add 2 equal parts of deionized water to the uniform solution, continue stirring for 1-2 hours, and stand for 8 minutes to obtain the PVDF-HFP passivation film precursor.

[0064] Step 2: Prepare a polytetrafluoroethylene-hexafluoropropylene passivation film: Use a scraper to evenly spread the above-obtained viscous PVDF-HFP passivation film precursor in a polytetrafluoroethylene mold, evaporate most of the acetone at room temperature, and then vacuum dry at 70°C for 36 hours to remove free solvent molecules to obtain a polytetrafluoroethylene-hexafluoropropylene passivation film, labeled as PVDF-HFP.

[0065] Step 3: Construct a LiF-rich modified layer on the surface of the lithium anode: Using a thermally driven method, the prepared passivation film PVDF-HFP is hot-pressed onto the surface of the lithium anode at 80°C and treated at a pressure of 1.0T for 1.5h to obtain a PVDF-HFP-modified lithium anode, labeled as PVDF-HFP@Li.

[0066] Step 4: First, 100 mg of Li6PS5Cl sulfide solid electrolyte powder was placed into a PEEK mold (diameter: 10 mm), and pressurized at a pressure of 1.4 T for 6 minutes to obtain a solid electrolyte layer.

[0067] Step 5: Place the lithium anode (diameter: 9 mm) processed in step 3 on both sides of the electrolyte layer prepared in step 4, and pressurize at 0.5T and maintain the pressure for 5 minutes. Finally, apply a constant pressure of 1T to the outer shell of the pressure mold to assemble a lithium-lithium symmetric battery, marked as PVDF-HFP@Li symmetric battery.

[0068] Comparative Example 2

[0069] The preparation method of the untreated-Li symmetric battery comprises the following steps:

[0070] Step 1: First, 100 mg of Li6PS5Cl sulfide solid electrolyte powder is placed into a polyetheretherketone (PEEK) mold (diameter: 10 mm), and pressurized and maintained at a pressure of 1.4 tons (T) for 5-10 minutes to obtain a solid electrolyte layer.

[0071] Step 2: Place untreated lithium anodes (diameter: 9 mm) on both sides of the electrolyte layer prepared in step 1, and pressurize at 0.5T and maintain the pressure for 5 minutes. Finally, apply a constant pressure of 1T to the outer shell of the pressure mold to assemble a lithium-lithium symmetric battery, marked as untreated-Li symmetric battery.

[0072] Comparative Example 3

[0073] The difference from Example 2 is that magnesium fluoride is first coated on the lithium anode, and then the PVDF-HFP passivation film is hot-pressed. The prepared symmetrical electrode is marked as PVDF-HFP-3%MgF2@Li.

[0074] The specific preparation process is as follows:

[0075] Step 1, preparation of polytetrafluoroethylene-hexafluoropropylene passivation film precursor: dissolve the PVDF-HFP after removing water in acetone in turn, wherein 0.97g of PVDF-HFP is dissolved in every 10ml of acetone. Stir magnetically for 10h at a speed of 500r / min and 50°C. After PVDF-HFP is completely dissolved, add deionized water to the uniform solution in the same amount as in Example 2, and continue stirring for 1.5h. After standing for 8min, a PVDF-HFP passivation film precursor is obtained.

[0076] Step 2: Preparation of polytetrafluoroethylene-hexafluoropropylene passivation film: Use a scraper to evenly spread the above-obtained viscous PVDF-HFP passivation film precursor in a polytetrafluoroethylene mold. After most of the acetone is volatilized at room temperature, vacuum dry at 70°C for 36 hours to remove free solvent molecules to obtain a polytetrafluoroethylene-hexafluoropropylene passivation film, which is labeled as PVDF-HFP.

[0077] Step 3: Constructing a LiF / Mg-rich modified layer on the surface of the lithium anode:

[0078] 0.03 g of magnesium fluoride was heated and stirred continuously to obtain a uniformly mixed molten solution, and the molten solution was coated on the lithium anode using a coater, and MgF2@Li was obtained after cooling;

[0079] The prepared passivation film PVDF-HFP was hot pressed onto the surface of the MgF2@Li anode at 80°C using a thermal driving method and treated at a pressure of 1.0 T for 1.5 h to obtain PVDF-HFP-3%MgF2@Li.

[0080] Step 4: Same as Example 2.

[0081] Step 5: Same as Example 2.

[0082] Comparative Example 4

[0083] The difference from Example 2 is that the total mass of PVDF-HFP and MgF2 added in step 1 is 100 equal parts, and the mass proportion of MgF2 is 10 equal parts. A 10% MgF2-PVDF-HFP@Li symmetric electrode is prepared.

[0084] Test example

[0085] The electrochemical performance of the symmetrical batteries of the embodiment and the comparative example was tested. The test results are shown in Table 1.

[0086] Table 1 Battery electrochemical performance test results

[0087]

[0088] As can be seen from the table above, the examples are much better than the comparative examples in terms of critical current density and cycle performance. In particular, the 3%MgF2-PVDF-HFP@Li symmetric battery exhibits an ultra-high CCD value (2.0 mA cm -2 ), which is 5 times that of pure lithium. In addition, the 3% MgF2-PVDF-HFP@Li symmetrical battery can stably perform lithium plating / stripping for more than 1500h, and the overpotential is reduced to 7.8mV. This shows that the 3% MgF2-PVDF-HFP@Li anode of the present invention has better lithium dendrite inhibition ability and interface compatibility, which enhances the advantages of 3% MgF2-PVDF-HFP@Li anode material in the preparation of all-solid-state lithium batteries. Considering its simple preparation process and low cost of raw materials used, it is shown that the MgF2-PVDF-HFP passivation film has great application prospects for modifying lithium metal anodes.

[0089] Therefore, the present invention adopts a multifunctional passivation film of the above structure for modifying lithium anode and its preparation method, and adopts the phase inversion method to prepare magnesium fluoride-polytetrafluoroethylene-hexafluoropropylene multifunctional passivation film, and the inorganic filler MgF2 can not only effectively adjust the pore size and crystallinity of the passivation film, but also react with PVDF-HFP passivator molecules and lithium anode to generate a multifunctional passivation layer rich in LiF / Mg in situ, thereby adjusting the uniform deposition behavior of lithium during the electroplating / stripping process and inhibiting the formation of dendrites. Under the synergistic effect of the LiF / Mg modification layer and the MgF2-PVDF-HFP intermediate passivation layer, the interfacial compatibility between the electrolyte and the lithium anode is effectively enhanced, thereby achieving a highly reversible cycle, and the lithium anode modified by the passivation film exhibits considerable electrochemical performance, and is considered to be an ideal all-solid-state lithium battery material.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A multifunctional passivation film for modifying a lithium anode, characterized in that: The invention comprises a lithium anode and a MgF2-PVDF-HFP passivation film hot-pressed on the surface of the lithium anode. The MgF2-PVDF-HFP passivation film comprises MgF2 and PVDF-HFP. During the hot-pressing process, the MgF2 and PVDF-HFP in the MgF2-PVDF-HFP passivation film trigger an in-situ reaction with the lithium in the lithium anode to generate a modified layer rich in LiF / Mg.

2. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 1, characterized in that: The following steps are involved: (1) Preparation of MgF2-PVDF-HFP passivation film precursor Dissolve PVDF-HFP and MgF2 in acetone in turn, heat and stir, and after PVDF-HFP and MgF2 are completely dissolved, a uniform solution is obtained, deionized water is added to the uniform solution, and stirring is continued. After standing, a MgF2-PVDF-HFP passivation film precursor is obtained; (2) Preparation of MgF2-PVDF-HFP passivation film The viscous MgF2-PVDF-HFP passivation film precursor is evenly spread in a polytetrafluoroethylene mold using a scraper, and most of the acetone is volatilized at room temperature, and then treated in a vacuum drying oven to remove free solvent molecules to obtain a magnesium fluoride-polyvinylidene fluoride-hexafluoropropylene passivation film, namely, a MgF2-PVDF-HFP passivation film; (3) Construction of LiF / Mg-rich passivation layer on the lithium anode surface The prepared MgF2-PVDF-HFP passivation film was hot pressed onto the surface of the lithium anode using a thermal driving method. After pressure treatment, a lithium anode modified with MgF2-PVDF-HFP was obtained, namely MgF2-PVDF-HFP@Li.

3. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: The PVDF-HFP and MgF2 in step (1) are both reagents that have been heated in vacuum to remove moisture.

4. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: The specific process of heating and stirring in step (1) is: magnetic stirring for 10-12 hours at a rotation speed of 400-600 r / min and 50° C.; the stirring time is continued for 1-2 hours; and the standing time is 5-10 minutes.

5. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: In step (1), the total mass of PVDF-HFP and MgF2 dissolved in every 10 mL of acetone is 1 g, wherein the mass ratio of PVDF-HFP to MgF2 is (96-100):(0-4).

6. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: In step (1), the volume ratio of the added amount of deionized water and acetone is 1:(8-10).

7. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: In step (2), the temperature of the vacuum drying oven is 60 to 80° C., and the treatment time is 24 to 48 hours.

8. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: In step (3), the hot pressing temperature is 70-90° C., the pressure is 0.8-1.4T, and the hot pressing time is 1-2h.

9. The method for preparing a multifunctional passivation film for modifying a lithium anode according to claim 2, characterized in that: All operations in step (3) were performed in a glove box filled with an inert atmosphere.

Citation Information

Patent Citations

  • Metal lithium negative electrode material, as well as preparation method and application thereof

    CN109950476A

  • Lithium metal negative electrode with double-layer interface film, preparation thereof and application

    CN111293283A

  • Interface layer and application thereof in battery

    CN116613397A

  • Lithium negative electrode modification method and battery thereof

    CN116791083A

  • Negative electrode for lithium secondary battery and method for producing same

    CN117425971A