Vanadium heptaoxide / carbon cloth flexible integrated negative electrode material and preparation method thereof
By growing a vanadium heptaoxide nanoflower structure on a carbon cloth substrate, it solves the problems of structural stability and low lithium ion diffusion rate in lithium-ion batteries, achieves high rate performance and flexibility, and is suitable for large-scale use.
Patent Information
- Application Number
- CN202411179010.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
As an electrode material for lithium-ion batteries, tetravanadium heptaoxide has problems with poor structural stability and low lithium ion diffusion rate, resulting in rapid capacity fading and poor stability, making it unable to be used on a large scale.
Using the preparation method of tetravanadium heptaoxide/carbon cloth flexible integrated anode material, active materials are grown on the carbon cloth substrate to form a nanoflower morphology structure, which shortens the diffusion path of lithium ions, improves electrochemical performance, and is cleaned by ultrasonic waves , magnetic stirring, hydrothermal reaction and vacuum drying and other steps to achieve self-supporting and flexible integration of the material.
The obtained material has excellent flexibility and high-rate performance, avoids the pulverization of active materials during the charge and discharge process, improves electrochemical performance, and is suitable for large-scale promotion and use.
Smart Images

Figure CN118738294A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a vanadium heptoxide / carbon cloth flexible integrated negative electrode material and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development of portable and flexible wearable electronic devices, flexible lithium-ion batteries have gradually attracted widespread attention from researchers. As one of the key components of flexible lithium-ion batteries, negative electrode materials have very high requirements for their high capacity, cycle stability and flexibility. At present, negative electrode materials for lithium-ion batteries are mainly divided into carbon-based materials, alloying reaction materials, metal oxides, metal sulfides, metal phosphides, etc. Metal oxides have attracted the attention of many researchers due to their high theoretical capacity. Among the many metal oxides, vanadium oxide (V x O y ) has been widely studied due to its rich valence states, high theoretical capacity, and low cost. As a type of vanadium oxide, tetravanadium heptoxide (V4O7) is currently used in liquid crystal displays, photocatalysis, electrocatalysis, lithium-ion batteries, aqueous zinc-ion batteries, and other fields. However, in the field of lithium-ion batteries, due to the poor structural stability and low lithium ion diffusion rate of tetravanadium heptoxide as an electrode material, its capacity decays quickly and its stability is poor, making it impossible to use it on a large scale. Currently, tetravanadium heptoxide is mostly prepared as solid powder. The powder is easy to detach from the current collector when the prepared electrode is folded and bent, and it is easy to pulverize during the charge and discharge reaction, resulting in serious capacity decay. Summary of the invention
[0003] The present invention provides a vanadium heptoxide / carbon cloth flexible integrated negative electrode material and a preparation method thereof, so as to solve the problems of poor structural stability and low lithium ion diffusion rate of vanadium heptoxide as an electrode material.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix deionized water, ethylene glycol and ammonium metavanadate in an ultrasonic cleaner; S2, immersing the mixed material into the pretreated carbon cloth and stirring with a magnetic stirrer; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a blast drying oven for heating, cool after heating, wash with anhydrous ethanol, and finally place in a vacuum drying oven for drying.
[0005] Preferably, in step S1, according to the mass-to-volume ratio, the volume of deionized water is 1.5-15 mL, the volume of ethylene glycol is 10-100 mL, the mass of ammonium metavanadate is 0.01-0.3 g, and the ultrasonic cleaning time is 0.5-5 h.
[0006] Preferably, in step S2, the pretreatment is to place the carbon in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 4-8 mol / L, the reaction temperature is 80-120 °C, and the reaction time is 2-4 h; the speed of the magnetic stirrer is set to 50-400 rpm, and the stirring time is 0.5-48 h.
[0007] Preferably, in step S3, the heating setting temperature of the blast drying oven is 200° C. and the heating time is 6 to 48 h.
[0008] Another technical solution adopted by the present invention is: a negative electrode material obtained by the preparation method of the present invention.
[0009] The beneficial effects of the present invention are: by in-situ growing active materials on a carbon cloth substrate, the self-supporting flexible integrated electrode obtained has excellent flexibility, can meet the needs of flexible batteries, and can also prevent the active materials from separating from the current collector during the electrochemical reaction, avoid the material from pulverizing during the charge and discharge reaction, and form a nanoflower morphology structure on carbon cloth (CC) by tetravanadium heptoxide, which can shorten the diffusion path of lithium ions, alleviate volume expansion, and avoid agglomeration of nanoparticles due to low thermodynamic stability, thereby further improving electrochemical performance. The lithium-ion battery made from the negative electrode material of the present invention has excellent rate performance, high charge and discharge capacity, and the method is simple and easy to operate, low cost, and suitable for large-scale promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0011] Figure 1 This is the XRD pattern of the flexible negative electrode prepared in Example 1 of the present invention; Figure 2 This is a SEM image of the flexible material prepared in Example 1 of the present invention with a scale of 20 μm; Figure 3 This is a SEM image of the flexible material prepared in Example 1 of the present invention with a scale of 5 μm; Figure 4 This is an EIS graph of the flexible material prepared in Example 1 of the present invention; Figure 5 This is a diagram showing the flexibility of the flexible negative electrode prepared in Example 1 of the present invention; Figure 6 is the XRD pattern of the negative electrode material prepared in Example 2 of the present invention; Figure 7 is a SEM image of the negative electrode material prepared in Example 2 of the present invention; Figure 8 This is the XRD pattern of the flexible negative electrode prepared in Example 4 of the present invention; Fig. 9 This is a SEM image of the flexible negative electrode prepared in Example 4 of the present invention; Fig.10 This is the XRD diagram of the flexible negative electrode prepared in Comparative Example 1 of the present invention; Fig.11 This is the XRD diagram of the flexible negative electrode prepared in Comparative Example 2 of the present invention; Fig.12 This is a SEM image of the flexible negative electrode prepared in Comparative Example 2 of the present invention; Fig.13 The flexible negative electrode prepared in Example 1 of the present invention is applied to the charging and discharging rate performance diagram of lithium-ion batteries at different current densities; Fig.14 This is a rate performance diagram of the negative electrode material prepared in Comparative Example 2 of the present invention when applied to a lithium-ion battery for charge and discharge at different current densities. DETAILED DESCRIPTION
[0012] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] Example 1
[0014] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 10 mL of deionized water, 70 mL of ethylene glycol and 0.1 g of ammonium metavanadate (NH4VO3) in an ultrasonic cleaner for 3 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 300 rpm, and stir for 18 h. The pretreatment is to place the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 6 mol / L, the reaction temperature is 100 °C, and the reaction time is 3 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 24 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0015] Its XRD Figure 1 As shown, at 2θ = 25.5 o and 43.6 o The two broad peaks that appear correspond to the diffraction peaks caused by the carbon cloth substrate. According to the JCPDS (Joint Committee on Powder Diffraction Standards) card number 03-065-6448, the peaks (001), (010), (002), (-101) and (1-11) correspond to the characteristic peaks caused by tetravanadium heptoxide. like Figure 2 As shown, it can be seen that vanadium heptoxide has completely covered the carbon cloth. like Figure 3 As shown, it can be seen that the morphology of tetravanadium heptoxide is nanoflower; like Figure 4 As shown, compared with vanadium heptoxide powder, the vanadium heptoxide / carbon cloth integrated material has a smaller semicircle diameter in the medium and high frequency regions of EIS (electrochemical impedance spectroscopy) and a smaller slope in the low frequency region. It can be seen that the vanadium heptoxide / carbon cloth self-supporting flexible electrode nanoflower structure has a smaller charge transfer impedance and better ion diffusion capacity. like Figure 5 As shown, a bending test was performed on the vanadium heptoxide / carbon cloth self-supporting flexible electrode prepared in Example 1, and it was found that the material had good flexibility.
[0016] Example 2
[0017] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 5 mL of deionized water, 35 mL of ethylene glycol, and 0.05 g of NH4VO3 in an ultrasonic cleaner for 1 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 200 rpm, stir for 6 h, pre-treat by placing the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 4 mol / L, the reaction temperature is 100 °C, and the reaction time is 3 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 12 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0018] Its XRD Figure 6 The scanning electron microscope image is shown in Figure 7 As shown, it can be seen that under the preparation conditions of this embodiment, the characteristic peaks of tetravanadium heptoxide and the morphological structure on the carbon cloth are nanorods.
[0019] Example 3
[0020] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 10 mL of deionized water, 70 mL of ethylene glycol and 0.1 g of NH4VO3 in an ultrasonic cleaner for 3 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 300 rpm, stir for 12 h, pre-treat by placing the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 6 mol / L, the reaction temperature is 100 °C, and the reaction time is 3 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 12 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0021] Example 4
[0022] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 10 mL of deionized water, 70 mL of ethylene glycol and 0.1 g of NH4VO3 in an ultrasonic cleaner for 3 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 300 rpm, and stir for 24 h; pretreatment is to place the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 6 mol / L, the reaction temperature is 100 ° C, and the reaction time is 3 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 36 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0023] In this example, XRD Figure 8 As shown in the scanning electron microscope image Fig. 9 As shown, the nanoflower structure can be clearly observed.
[0024] Example 5
[0025] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 10 mL of deionized water, 70 mL of ethylene glycol and 0.2 g of NH4VO3 in an ultrasonic cleaner for 3 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 300 rpm, stir for 24 h, pre-treat by placing the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 6 mol / L, the reaction temperature is 100 °C, and the reaction time is 3 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 48 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0026] Example 6
[0027] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 1.5 mL of deionized water, 10 mL of ethylene glycol, and 0.01 g of NH4VO3 in an ultrasonic cleaner for 0.5 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 50 rpm, stir for 0.5 h, pre-treat the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 4 mol / L, the reaction temperature is 80 ° C, and the reaction time is 4 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 6 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0028] Example 7
[0029] A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: S1. Mix 15 mL of deionized water, 100 mL of ethylene glycol and 0.3 g of NH4VO3 in an ultrasonic cleaner for 5 h. S2, after mixing, immerse in pretreated carbon cloth, stir with a magnetic stirrer, set the speed of the magnetic stirrer to 400 rpm, stir for 48 h, pre-treat by placing the carbon cloth in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 8 mol / L, the reaction temperature is 120 °C, and the reaction time is 2 h; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a forced air drying oven for heating, set the temperature to 200 °C, and heat for 48 h; after heating, cool to room temperature (25 °C), wash with anhydrous ethanol, and place in a vacuum drying oven for drying.
[0030] Comparative Example 1: A method for preparing a vanadium heptoxide negative electrode material comprises the following steps: (1) Mix 5 mL of deionized water, 35 mL of ethylene glycol, and 0.05 g of NH4VO3 in an ultrasonic cleaner for 1 h. (2) After stirring, the mixture was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated in a forced air drying oven at 200 °C for 12 h. After heating, the mixture was cooled to room temperature (25 °C) and then centrifuged to obtain vanadium heptoxide powder, which was washed with anhydrous ethanol and dried in a vacuum drying oven.
[0031] The XRD of this comparative example is Fig.10 shown.
[0032] Comparative Example 2: A method for preparing a vanadium heptoxide negative electrode material comprises the following steps: (1) Mix 5 mL of deionized water, 35 mL of ethylene glycol, and 0.05 g of NH4VO3 in an ultrasonic cleaner for 1 h. (2) After stirring, the mixture was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated in a forced air drying oven at 200 °C for 24 h. After heating, the mixture was cooled to room temperature (25 °C) and then centrifuged to obtain vanadium heptoxide powder, which was washed with anhydrous ethanol and dried in a vacuum drying oven.
[0033] The XRD of this comparative example is Fig.11 As shown in the scanning electron microscope image Fig.12 As shown, the EIS diagram is Figure 3 As shown, without adding carbon cloth, the vanadium heptoxide powder is in a clamshell shape, which is not conducive to the diffusion of lithium ions.
[0034] Comparative Example 3: A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: (1) Mix 10 mL of deionized water, 70 mL of ethylene glycol, and 0.1 g of NH4VO3 in an ultrasonic cleaner for 3 h. (2) After mixing, immerse in the pretreated nickel foam and stir with a magnetic stirrer. The speed of the magnetic stirrer is set at 300 rpm and the stirring time is 18 h. (3) After stirring, transfer the mixture to a stainless steel autoclave lined with polytetrafluoroethylene and heat it in a forced air drying oven at 200 °C for 24 h. After heating, cool the mixture to room temperature (25 °C), wash it with anhydrous ethanol, and dry it in a vacuum drying oven.
[0035] In this comparative example, nickel foam is selected as a carrier, but because of its brittle material, it is not suitable as a flexible electrode, and the product is doped with metal ions during the synthesis process, resulting in an impure product.
[0036] Comparative Example 4: A method for preparing a vanadium heptoxide / carbon cloth flexible integrated negative electrode material comprises the following steps: Mix 10 mL of deionized water, 70 mL of ethylene glycol, and 1 g of NH4VO3 in an ultrasonic cleaner for 3 h.
[0037] This comparative example uses 1 g of NH4VO3, and NH4VO3 cannot be completely dissolved during the preparation process.
[0038] The negative electrode materials provided in the above Example 1 and Comparative Example 2 were assembled into batteries for charge and discharge tests. The battery composition is as follows: the positive electrode is a lithium sheet; the electrolyte is a mixture of EC, DEC and EMC, with a volume ratio of 1:1:1; the separator is a Celgard2600 microporous polypropylene membrane, and assembled into a CR2016 model battery. The types of the electrodes, separators and electrolytes can be replaced by other products.
[0039] Test conditions: The test was conducted using the CT2001A battery test system of Wuhan Blue Electric Electronics Co., Ltd. The temperature was room temperature (25 °C) and the current density selection range was 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 8 Ag -1 ), the charge and discharge voltage is limited to 0.01~3 V, and constant current charge and discharge experiments are carried out.
[0040] like Fig.13 As shown, the vanadium heptoxide / carbon cloth self-supporting flexible integrated negative electrode obtained in Example 1 is 0.1 Ag -1 and 8 Ag -1 The specific capacities of the battery can reach 1277.1 mAh / g and 136.2 mAh / g under different current densities, respectively, indicating excellent rate performance.
[0041] like Fig.14 As shown, the vanadium heptoxide powder negative electrode obtained in Comparative Example 2 is 0.1 Ag -1 and 4 Ag -1 When charged and discharged at the current density, its specific capacity is only 530.8 mAh / g and 47.8 mAh / g. It can be seen that the vanadium heptoxide / carbon cloth self-supporting flexible integrated negative electrode in this application has obvious improvement in rate performance compared with the vanadium heptoxide powder negative electrode, and the composite with carbon cloth improves the electrochemical performance.
[0042] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A method for preparing a flexible integrated negative electrode material of tetravanadium heptoxide / carbon cloth, It is characterized in that The following steps are involved: S1. Mix deionized water, ethylene glycol and ammonium metavanadate in an ultrasonic cleaner; S2, immersing the mixed material into the pretreated carbon cloth and stirring with a magnetic stirrer; S3. After stirring, transfer to a stainless steel autoclave lined with polytetrafluoroethylene, place in a blast drying oven for heating, cool after heating, wash with anhydrous ethanol, and finally place in a vacuum drying oven for drying.
2. The method for preparing the vanadium heptoxide / carbon cloth flexible integrated negative electrode material according to claim 1, It is characterized in that In the step S1, according to the mass-to-volume ratio, the volume of deionized water is selected to be 1.5-15 mL, the volume of ethylene glycol is selected to be 10-100 mL, and the mass of ammonium metavanadate is selected to be 0.01-0.3 g; and the ultrasonic time of the ultrasonic cleaner is selected to be 0.5-5 h.
3. The method for preparing the vanadium heptoxide / carbon cloth flexible integrated negative electrode material according to claim 1, It is characterized in that In step S2, the pretreatment process is to place the carbon in a nitric acid aqueous solution for hydrothermal reaction, the concentration of the nitric acid aqueous solution is 4-8 mol / L, the reaction temperature is 80-120 ° C, and the reaction time is 2-4 h; The magnetic stirrer was set at a speed of 50-400 rpm and a stirring time of 0.5-48 h.
4. The method for preparing the vanadium heptoxide / carbon cloth flexible integrated negative electrode material according to claim 1, It is characterized in that In step S3, the heating temperature of the blast drying oven is 200° C. and the heating time is 6 to 48 hours.
5. A vanadium heptoxide / carbon cloth flexible integrated negative electrode material, It is characterized in that The vanadium heptoxide / carbon cloth flexible integrated negative electrode material is obtained by the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Aluminum secondary battery vanadium oxide positive material and preparation method thereof
CN105304885A
Multi-valence-state vanadium oxide flexible electrode preparation method