Composite negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery
By using nanodiamond-coated graphite anode materials in lithium-ion batteries, the problem of poor structural stability of graphite anode materials is solved, the rate performance and cycle stability of lithium-ion batteries are improved, and rapid lithium ion transmission and high energy are achieved density.
Patent Information
- Application Number
- CN202410813914.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
The graphite anode material in existing lithium-ion batteries has a high degree of crystallization and poor structural stability, resulting in poor high-current charge and discharge performance, poor rate performance and cycle life.
Using nanodiamond as the coating layer, the nanodiamond coating layer is formed on the graphite surface to provide more lithium ion adsorption sites, improve the lithium ion transmission speed and the specific surface area of the negative electrode material, and enhance the rate performance and cycle stability.
Through the use of nanodiamond coatings, the rate performance and cycle stability of lithium-ion batteries are significantly improved, lithium deposition is avoided, and the fast charging capability and energy density of the battery are improved.
Smart Images

Figure CN118738332A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite negative electrode material and a preparation method thereof, a negative electrode sheet and a lithium ion battery. Background Art
[0002] At present, graphite has become the most widely used negative electrode material in lithium-ion batteries due to its advantages such as abundant resources, low price, low charge and discharge voltage platform and good safety.
[0003] However, graphite has a high degree of crystallization, poor structural stability, and poor compatibility with the electrolyte. In addition, due to the low diffusion rate of lithium ions in its ordered layered structure, the material has poor high-current charge and discharge performance and is prone to lithium precipitation, resulting in poor rate performance and a significantly reduced cycle life.
[0004] In view of this, there is an urgent need to develop a composite negative electrode material that can take into account battery rate performance while ensuring cycle stability. Summary of the invention
[0005] The purpose of the present invention is to provide a composite negative electrode material to effectively improve the rate performance and cycle stability of a battery in view of the deficiencies of the prior art.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A composite negative electrode material comprises a core and a coating layer coated on the outer surface of the core, wherein the core is graphite and the coating layer is nano-diamond.
[0008] Among them, nanodiamond has properties such as high lithium adsorption capacity, low expansion coefficient and large specific surface area. Introducing nanodiamond particles into the surface coating layer of graphite negative electrode materials can provide more lithium ion adsorption sites, realize rapid lithium ion transmission, and improve the battery's rate performance and cycle stability. The strong adsorption capacity of nanodiamond for lithium ions can induce lithium ions to better embed into the negative electrode and avoid the generation of lithium deposition.
[0009] Preferably, the graphite has a particle size D50 of 8-20 μm and a specific surface area of 0.8-4.0 m 2 / g, compacted density is 1.5-2.0cm 3 / g, gram capacity is greater than or equal to 335mAh / g. Graphite is the core of the composite negative electrode material and provides lithium storage. When the graphite particle size D50 is less than 8μm, it causes the compaction loss of the pole piece and reduces the energy density of the battery cell. When the graphite particle size D50 is greater than 20μm, the path of lithium ion embedding in graphite is too long, which deteriorates the fast charging performance of the battery cell.
[0010] Preferably, the particle size D50 of the nano-diamond is 5-100 nm.
[0011] Preferably, the nanodiamond includes one or more of natural nanodiamond, nanodiamond modified with oxygen groups, nanodiamond modified with nitrogen groups, and nanodiamond modified with phosphorus groups.
[0012] In addition, the present invention also provides a method for preparing a composite negative electrode material, comprising the following steps:
[0013] Step S1, dispersing nanodiamonds in a liquid coating agent to obtain a nanodiamond liquid coating agent;
[0014] Step S2, mixing graphite with the nano-diamond liquid phase coating agent obtained in step S1 to obtain a precursor;
[0015] Step S3, placing the precursor obtained in step S2 in an inert atmosphere for carbonization treatment, and cooling, to obtain the composite negative electrode material.
[0016] Preferably, in step S1, the mass ratio of the nanodiamond to the liquid-phase coating agent is 1:(20-100). When the mass ratio of the nanodiamond to the liquid-phase coating agent is less than 1:100, the content of nanodiamonds in the graphite coating layer will be too low and unevenly distributed, and the effect of improving the fast charging performance will not be obvious; when the mass ratio of the nanodiamond to the liquid-phase coating agent is greater than 1:20, the content of nanodiamonds in the graphite coating layer will be too high, resulting in an excessively high specific surface area of the composite negative electrode, which will deteriorate the first effect. More preferably, in step S1, the mass ratio of the nanodiamond to the liquid-phase coating agent is 1:(50-80).
[0017] Preferably, in step S1, the liquid coating agent is a mixture of one or more of heterocyclic aromatic hydrocarbons, ketones, hydrocarbons, resins, petroleum asphalt, and coal tar; the viscosity of the liquid coating agent is 20-100 mPa·s, and the residual carbon value is 5-40%.
[0018] Preferably, in step S1, the dispersion method is ultrasonic dispersion, the ultrasonic frequency is 30-80 Hz, the power is 2000-3000 W, and the ultrasonic stirring time is 0.5-5 h.
[0019] Preferably, in step S2, the mass ratio of the nano-diamond liquid-phase coating agent to the graphite is (1-10):100; more preferably, in step S2, the mass ratio of the nano-diamond liquid-phase coating agent to the graphite is (3-8):100.
[0020] Preferably, in step S3, the temperature of the carbonization treatment is 900-1200°C, the heating time is 9-15h, the heat preservation time is 5-8h, and the cooling time is 6-12h.
[0021] In addition, the present invention also provides a negative electrode sheet, comprising the above-mentioned composite negative electrode material.
[0022] In addition, the present invention also provides a lithium-ion battery, including a battery cell formed by winding a negative electrode sheet, a positive electrode sheet and a separator, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the negative electrode sheet is the above-mentioned negative electrode sheet.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adds nano-diamond components to the liquid phase coating agent, and realizes high-strength bonding between nano-diamond particles and the graphite surface through liquid phase coating to form a dense nano-diamond coating layer, thereby providing more lithium ion adsorption sites for the graphite surface coating layer, accelerating the lithium ion transmission speed, and improving the specific surface area, rate performance and cycle performance of the negative electrode material, thereby improving the rate performance and cycle stability of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of the composite negative electrode material of Example 1 of the present invention.
[0025] Figure 2 This is a SEM image of the composite negative electrode material of Example 1 of the present invention.
[0026] Among them, 1-core; 2-cladding layer. DETAILED DESCRIPTION
[0027] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] According to a first aspect of the present application, the present application provides a composite negative electrode material, comprising a core and a coating layer coated on the outer surface of the core, wherein the core is graphite and the coating layer is nanodiamond.
[0029] In some embodiments, the particle size D50 of graphite is 8-20 μm, preferably 10-15 μm. For example, it can be 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm. The specific surface area of graphite is 0.8-4.0 m 2 / g, preferably 1.0 to 2.0 m 2 / g. For example, it can be 0.8m 2 / g, 1.0m2 / g, 1.8m 2 / g, 2.0m 2 / g, 2.8m 2 / g, 3.0m 2 / g, 3.8m 2 / g, 4.0m 2 / g. The compacted density of graphite is 1.5-2.0cm 3 / g, preferably 1.70 to 1.80 cm 3 / g. For example, it can be 1.5cm 3 / g, 1.6cm 3 / g, 1.7cm 3 / g, 1.8cm 3 / g, 1.9cm 3 / g, 2.0cm 3 / g.
[0030] In some embodiments, the gram capacity of graphite is greater than or equal to 335 mAh / g, preferably 350 to 360 mAh / g, for example, 335 mAh / g, 345 mAh / g, 355 mAh / g, 365 mAh / g, or 375 mAh / g.
[0031] In some embodiments, the graphite includes one or more of needle coke, petroleum coke, and pitch coke. The graphite particle structure can be a single particle structure, a secondary particle structure, or multiple ratios of the two.
[0032] In some embodiments, the particle size D50 of the nanodiamond is 5-100 nm, for example, 5 nm, 15 nm, 25 nm, 35 nm, 45 nm, 55 nm, 65 nm, 75 nm, 85 nm, 95 nm, 100 nm. In some embodiments, the nanodiamond includes one or more of natural nanodiamond, nanodiamond modified with oxygen groups, nanodiamond modified with nitrogen groups, and nanodiamond modified with phosphorus groups.
[0033] According to a second aspect of the present application, the present application provides a method for preparing a composite negative electrode material, comprising the following steps:
[0034] Step S1, dispersing nanodiamonds in a liquid coating agent by ultrasonication to obtain a nanodiamond liquid coating agent;
[0035] Step S2, mixing graphite with the nano-diamond liquid phase coating agent obtained in step S1 to obtain a precursor;
[0036] Step S3, placing the precursor obtained in step S2 in an inert atmosphere for carbonization treatment, and cooling, to obtain the composite negative electrode material.
[0037] Among them, ultrasonic stirring can make nanodiamonds pre-dispersed in the liquid coating agent, and in the mechanical fusion process, nanodiamonds are evenly distributed on the graphite surface along with the liquid coating agent. Adding nanodiamonds to the liquid coating agent can provide more lithium ion adsorption sites for the graphite surface coating layer, realize rapid lithium ion transmission, and improve the battery's rate performance and cycle stability.
[0038] In some embodiments, in step S1, the mass ratio of nanodiamond to liquid coating agent is 1:(20-100), for example, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100. More preferably, in step S1, the mass ratio of nanodiamond to liquid coating agent is 1:(50-80).
[0039] In some embodiments, in step S1, the liquid coating agent is a mixture of one or more of heterocyclic aromatic hydrocarbons, ketones, hydrocarbons, resins, petroleum asphalt, and coal tar. The viscosity of the liquid coating agent is 20 to 100 mPa·s, for example, it can be 20 mPa·s, 30 mPa·s, 40 mPa·s, 50 mPa·s, 60 mPa·s, 70 mPa·s, 80 mPa·s, 90 mPa·s, 100 mPa·s. The residual carbon value of the liquid coating agent is 5 to 40%, for example, it can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%.
[0040] In some embodiments, in step S1, the ultrasonic dispersion frequency is 30-80 Hz, for example, 30 Hz, 40 Hz, 50 Hz, 60 Hz, 70 Hz, 80 Hz. The power is 2000-3000 W, for example, 2000 W, 2100 W, 2200 W, 2300 W, 2400 W, 2500 W, 2600 W, 2700 W, 2800 W, 2900 W, 3000 W. The ultrasonic stirring time is 0.5-5 h, for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h.
[0041] In some embodiments, in step S2, the mass ratio of the nano-diamond liquid-phase coating agent to the graphite is (1-10):100, for example, 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100. If the mass ratio of the nano-diamond liquid-phase coating agent to the graphite is greater than the set range, the negative electrode material gram capacity will be reduced, thereby reducing the battery energy density. More preferably, in step S2, the mass ratio of the nano-diamond liquid-phase coating agent to the graphite is (3-8):100.
[0042] In some embodiments, in step S2, the nano-diamond liquid phase coating agent and graphite are mixed in a fusion machine, wherein the fusion machine is a mechanical fusion machine with a cooling water interlayer.
[0043] In some embodiments, in step S3, the carbonization treatment temperature is 900-1200°C, for example, 900°C, 1000°C, 1100°C, 1200°C. The heating time is 9-15h, for example, 9h, 10h, 11h, 12h, 13h, 14h, 15h. The heat preservation time is 5-8h, for example, 5h, 6h, 7h, 8h. The cooling time is 6-12h, for example, 6h, 7h, 8h, 9h, 10h, 11h, 12h.
[0044] According to a third aspect of the present application, the present application provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer comprises the above-mentioned composite negative electrode material.
[0045] According to the fourth aspect of the present application, the present application provides a lithium-ion battery, comprising a battery cell formed by winding a negative electrode sheet, a positive electrode sheet and a separator, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the negative electrode sheet is the above-mentioned negative electrode sheet.
[0046] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material may include but is not limited to a chemical formula such as Li a Ni x Co y M z O 2-b N b (wherein 0.95≤a≤1.2, x>0, y≥0, z≥0, and x+y+z=1, 0≤b≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO 2 、LiNiO 2 、LiVO 2 、LiCrO 2 、LiMn 2 O 4 、LiCoMnO 4 , Li 2 NiMn 3 O 8 、LiNi 0.5 Mn 1.5 O 4 、LiCoPO4 、LiMnPO 4 、LiFePO 4 、LiNiPO 4 、LiCoFSO 4 , CuS 2 , FeS 2 、MoS 2 、NiS、TiS 2 The positive electrode active material may also be subjected to a modification treatment. The method for modifying the positive electrode active material should be known to those skilled in the art. For example, the positive electrode active material may be modified by coating, doping, etc. The material used for the modification treatment may include but is not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc. The positive electrode current collector is usually a structure or part for collecting current. The positive electrode current collector may be any material suitable for use as a positive electrode current collector for lithium-ion batteries in the art. For example, the positive electrode current collector may include but is not limited to metal foil, etc., and more specifically may include but is not limited to aluminum foil, etc.
[0047] The separator can be any material suitable for secondary battery separators in the art, for example, it can be a combination of one or more of, but not limited to, polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers.
[0048] The lithium-ion battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. The electrolyte lithium salt can be LiPF used in high-temperature electrolytes. 6 and / or LiBOB; it can also be LiBF used in low temperature electrolytes 4 、LiBOB、LiPF 6 It can also be LiBF used in the overcharge-proof electrolyte 4 、LiBOB、LiPF 6 , LiTFSI; it can also be LiClO 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2At least one of the above. The organic solvent may be a cyclic carbonate, including PC, EC; it may also be a chain carbonate, including DFC, DMC, or EMC; it may also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to film-forming additives, conductive additives, flame retardant additives, overcharge prevention additives, and additives for controlling H in the electrolyte. 2 At least one of an additive for increasing the content of O and HF, an additive for improving low temperature performance, and a multifunctional additive.
[0049] The present invention will be described in further detail below in conjunction with specific implementation modes, but the implementation modes of the present invention are not limited thereto.
[0050] Example 1
[0051] Negative electrode material preparation:
[0052] like Figures 1-2 As shown, a composite negative electrode material provided in this embodiment includes a core 1 and a coating layer 2 coated on the outer surface of the core 1, the core 1 is graphite, and the coating layer 2 is nanodiamond.
[0053] The method for preparing the composite negative electrode material comprises the following steps:
[0054] Step S1, disperse nanodiamond with a particle size D50 of 5 nm and liquid phenolic resin with a viscosity of 30 mPa·s and a residual carbon value of 12% in an ultrasonic reactor at a weight ratio of 1:50 to obtain a nanodiamond liquid coating agent, wherein the ultrasonic frequency is 40 Hz, the power is 2000 W, and the ultrasonic stirring time is 1 hour.
[0055] Step S2: the particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.70cm 3 / g of artificial graphite and the nano-diamond liquid phase coating agent obtained in step S1 are mixed in a fusion machine at a weight ratio of 100:3 to obtain a precursor. The rotation speed of the fusion machine is 600r / min, the temperature is 50°C, and the mixing time is 30min.
[0056] Step S3: put the precursor obtained in step S2 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a composite negative electrode material. The carbonization temperature is controlled at 1000°C, the heating time is 10 hours, and the cooling time is 8 hours.
[0057] Preparation of lithium-ion batteries:
[0058] 1) Positive electrode preparation: Lithium cobalt oxide (charging cut-off voltage greater than 4.48V), conductive carbon, and adhesive (polyvinylidene fluoride) are mixed evenly in N-methylpyrrolidone solvent at a mass ratio of 97.6:1.1:1.3 to form a positive electrode slurry, which is then coated on aluminum foil and dried, then cold pressed and slit to form a positive electrode sheet.
[0059] 2) Negative electrode sheeting: The composite negative electrode material, CMC and SBR prepared above were mixed evenly in deionized water at a mass ratio of 97.7:1.1:1.2 to prepare negative electrode slurry, which was then coated on copper foil and dried before being cold pressed and slit to prepare negative electrode sheets.
[0060] 3) Battery production: The above-mentioned positive electrode sheet, conventional separator, and negative electrode sheet are wound into a battery cell, the positive electrode is spot-welded with an aluminum tab, and the negative electrode is spot-welded with a nickel tab; then the battery cell is placed in an aluminum-plastic packaging bag, injected with a high-voltage electrolyte, and manufactured into a battery through the processes of packaging, formation, and capacity division.
[0061] Example 2
[0062] Different from Example 1, the method for preparing the composite negative electrode material in this embodiment includes the following steps:
[0063] Step S1, disperse nanodiamond with a particle size D50 of 7 nm and liquid coumarone resin with a viscosity of 50 mPa·s and a residual carbon value of 25% in an ultrasonic reactor at a weight ratio of 1:60 to obtain a nanodiamond liquid phase coating agent, wherein the ultrasonic frequency is 50 Hz, the power is 2200 W, and the ultrasonic stirring time is 1.5 h.
[0064] Step S2: the particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.61cm 3 / g of artificial graphite and the nano-diamond liquid phase coating agent obtained in step S1 are mixed in a fusion machine at a weight ratio of 100:4 to obtain a precursor. The rotation speed of the fusion machine is 700r / min, the temperature is 50°C, and the mixing time is 20min.
[0065] Step S3: put the precursor obtained in step S2 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a composite negative electrode material. The carbonization temperature is controlled at 1100°C, the heating time is 12 hours, and the cooling time is 10 hours.
[0066] The rest is the same as Example 1 and will not be described again here.
[0067] Example 3
[0068] Different from Example 1, the method for preparing the composite negative electrode material in this embodiment includes the following steps:
[0069] Step S1, disperse nanodiamond with a particle size D50 of 10 nm and liquid furfural resin with a viscosity of 40 mPa·s and a residual carbon value of 50% in an ultrasonic reactor at a weight ratio of 1:70 to obtain a nanodiamond liquid phase coating agent, wherein the ultrasonic frequency is 50 Hz, the power is 2200 W, and the ultrasonic stirring time is 2 hours.
[0070] Step S2: the particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.63cm 3 / g of artificial graphite and the nano-diamond liquid phase coating agent obtained in step S1 are mixed in a fusion machine at a weight ratio of 100:6 to obtain a precursor. The rotation speed of the fusion machine is 800r / min, the temperature is 50°C, and the mixing time is 15min.
[0071] Step S3: put the precursor obtained in step S2 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a composite negative electrode material. The carbonization temperature is controlled at 1150°C, the heating time is 13 hours, and the cooling time is 10 hours.
[0072] The rest is the same as Example 1 and will not be described again here.
[0073] Example 4
[0074] Different from Example 1, the method for preparing the composite negative electrode material in this embodiment includes the following steps:
[0075] Step S1, disperse nanodiamond with a particle size D50 of 15 nm and liquid petroleum asphalt with a viscosity of 100 mPa·s and a residual carbon value of 60% in an ultrasonic reactor at a weight ratio of 1:80 to obtain a nanodiamond liquid phase coating agent, wherein the ultrasonic frequency is 50 Hz, the power is 2200 W, and the ultrasonic stirring time is 2.5 h.
[0076] Step S2: the particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.62cm 3 / g of artificial graphite and the nano-diamond liquid phase coating agent obtained in step S1 are mixed in a fusion machine at a weight ratio of 100:8 to obtain a precursor. The rotation speed of the fusion machine is 1000r / min, the temperature is 50°C, and the mixing time is 10min.
[0077] Step S3: put the precursor obtained in step S2 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a composite negative electrode material. The carbonization temperature is controlled at 1200°C, the heating time is 15 hours, and the cooling time is 10 hours.
[0078] The rest is the same as Example 1 and will not be described again here.
[0079] Example 5
[0080] Different from Example 1, in step S1 of this example, the mass ratio of nano-diamond to liquid phenolic resin as a liquid coating agent is 1:20.
[0081] The rest is the same as Example 1 and will not be described again here.
[0082] Example 6
[0083] Different from Example 1, in step S1 of this example, the mass ratio of nano-diamond to liquid phenolic resin as a liquid coating agent is 1:15.
[0084] The rest is the same as Example 1 and will not be described again here.
[0085] Example 7
[0086] Different from Example 1, in step S1 of this example, the mass ratio of nano-diamond to liquid phenolic resin as a liquid coating agent is 1:100.
[0087] The rest is the same as Example 1 and will not be described again here.
[0088] Example 8
[0089] Different from Example 1, in step S1 of this example, the mass ratio of nano-diamond to liquid phenolic resin as a liquid coating agent is 1:105.
[0090] The rest is the same as Example 1 and will not be described again here.
[0091] Example 9
[0092] Different from Example 1, in step S2 of this example, the mass ratio of the nano-diamond liquid phase coating agent to graphite is 1:100.
[0093] The rest is the same as Example 1 and will not be described again here.
[0094] Example 10
[0095] Different from Example 1, in step S2 of this example, the mass ratio of the nano-diamond liquid phase coating agent to graphite is 1:10.
[0096] The rest is the same as Example 1 and will not be described again here.
[0097] Embodiment 11
[0098] Different from Example 1, in step S2 of this example, the mass ratio of the nano-diamond liquid phase coating agent to graphite is 0.5:100.
[0099] The rest is the same as Example 1 and will not be described again here.
[0100] Example 12
[0101] Different from Example 1, in step S2 of this example, the mass ratio of the nano-diamond liquid phase coating agent to graphite is 15:100.
[0102] The rest is the same as Example 1 and will not be described again here.
[0103] Embodiment 13
[0104] Different from Example 1, the particle size D50 of the artificial graphite in step S1 of this example is 25 μm.
[0105] The rest is the same as Example 1 and will not be described again here.
[0106] Comparative Example 1
[0107] Different from Example 1, the negative electrode material of this comparative example is a graphite negative electrode material without a nano-diamond coating layer.
[0108] The preparation method of the graphite negative electrode material of this comparative example comprises the following steps:
[0109] Step S1: The particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.70cm 3 / g of artificial graphite and liquid phenolic resin with a viscosity of 30mPa·s and a residual carbon value of 12% are mixed in a fusion machine at a weight ratio of 100:3 to obtain a precursor. The rotation speed of the fusion machine is 600r / min, the temperature is 50°C, and the mixing time is 30min.
[0110] Step S2: put the precursor obtained in step S1 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a graphite negative electrode material. The carbonization temperature is controlled at 1000°C, the heating time is 10 hours, and the cooling time is 8 hours.
[0111] The rest is the same as Example 1 and will not be described again here.
[0112] Comparative Example 2
[0113] Different from Example 2, the negative electrode material of this comparative example is a graphite negative electrode material without a nano-diamond coating layer.
[0114] The preparation method of the graphite negative electrode material of this comparative example comprises the following steps:
[0115] Step S1: The particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.61cm 3 / g of artificial graphite and liquid furfural resin with a viscosity of 50mPa·s and a residual carbon value of 25% are mixed in a fusion machine at a weight ratio of 100:4 to obtain a precursor. The rotation speed of the fusion machine is 700r / min, the temperature is 50°C, and the mixing time is 20min.
[0116] Step S2: put the precursor obtained in step S1 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a graphite negative electrode material. The carbonization temperature is controlled at 1100°C, the heating time is 12 hours, and the cooling time is 10 hours.
[0117] The rest is the same as Example 2 and will not be described again here.
[0118] Comparative Example 3
[0119] Different from Example 3, the negative electrode material of this comparative example is a graphite negative electrode material without a nano-diamond coating layer.
[0120] The preparation method of the graphite negative electrode material of this comparative example comprises the following steps:
[0121] Step S1: The particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.63cm 3 / g artificial graphite and liquid furfural resin with a viscosity of 40mPa·s and a residual carbon value of 50% are mixed in a fusion machine at a weight ratio of 100:6 to obtain a precursor. The rotation speed of the fusion machine is 800r / min, the temperature is 50°C, and the mixing time is 15min.
[0122] Step S2: put the precursor obtained in step S1 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a graphite negative electrode material. The carbonization temperature is controlled at 1150°C, the heating time is 13 hours, and the cooling time is 10 hours.
[0123] The rest is the same as Example 3 and will not be described again here.
[0124] Comparative Example 4
[0125] Different from Example 4, the negative electrode material of this comparative example is a graphite negative electrode material without a nano-diamond coating layer.
[0126] The preparation method of the graphite negative electrode material of this comparative example comprises the following steps:
[0127] Step S1: The particle size D50 is 11 μm, the gram capacity is 350 mAh / g, and the specific surface area is 2 m 2 / g, compacted density is 1.62cm 3 / g of artificial graphite and liquid petroleum asphalt with a viscosity of 100mPa·s and a residual carbon value of 60% are mixed in a fusion machine at a weight ratio of 100:8 to obtain a precursor. The rotation speed of the fusion machine is 800r / min, the temperature is 50°C, and the mixing time is 15min.
[0128] Step S2: put the precursor obtained in step S1 into a cartridge and place it in a carbonization furnace, perform carbonization treatment in a nitrogen atmosphere, cool it, and sieve it to obtain a graphite negative electrode material. The carbonization temperature is controlled at 1200°C, the heating time is 15 hours, and the cooling time is 8 hours.
[0129] The rest is the same as that of Example 4 and will not be described again here.
[0130] Performance Testing
[0131] 1. Gram capacity and first coulomb rate test: Using NMP (N-methylpyrrolidone) as solvent, each group of materials was mixed with SP (conductive carbon) and PVDF (polyvinylidene fluoride) at a mass ratio of 93:3:4 to make slurry, and then coated on a copper foil with a thickness of 6um, and the temperature was controlled at 100±5℃, and baked for 4 hours to obtain a pole piece, and then the pole piece was punched into a pole piece with a diameter of 20mm and assembled with a lithium sheet of the same diameter in a glove box to form a button battery, and the electrolyte used was a conventional electrolyte. The difference between the button batteries made by each group is only the different negative electrode materials used in the pole piece slurry. The test process of the button battery is carried out according to the following parameters in the industry standard, and the test process is not repeated: 0.05mA DC to 5mV, 0.1C CC to 2V.
[0132] 2. Rate test: In order to conduct rate test, the negative electrode materials of each group are first prepared into slurry, in which the negative electrode material: binder: dispersant = 97.7%: 0.5%: 0.6%, to make anode pole pieces, which are then wound with cathode pole pieces and separators into battery cells. After steps such as liquid injection and chemical composition, the finished battery cells are obtained. The difference between the finished battery cells obtained by each group is only the difference in the negative electrode materials used in the anode pole pieces. The finished battery cells are tested for lithium precipitation window with reference to the following parameters. The test method is specified by the industry standard and will not be repeated here: At room temperature, 6.0C / 6.5C / 7.0C / 7.5C CC to 4.45V, CV 0.05C; 1C DC to 3.0V are cycled for 20 weeks to obtain the battery cell lithium precipitation window data.
[0133] Method for measuring the compaction density of the negative electrode material: a compaction density meter (CARVER, USA) was used to measure the negative electrode materials of the embodiments and comparative examples according to the graphite negative electrode material powder compaction test method GB / T24533-2019, and the 5T compaction density value was recorded.
[0134] The lithium ion batteries prepared in the embodiment and the comparative example were respectively subjected to electrochemical performance tests. The test results are shown in Table 1.
[0135] Table 1
[0136]
[0137]
[0138]
[0139] From the comparison of the experimental data of Examples 1-13 and Comparative Examples 1-4 in Table 1, it can be seen that after adding nanodiamonds to the graphite coating layer, the compaction of the negative electrode material can be effectively improved, and the charging window is also significantly improved. The nanodiamonds provide more lithium ion adsorption sites for the graphite surface coating layer, realizing rapid lithium ion transmission, thereby increasing the lithium ion embedding speed and improving the fast charging capability.
[0140] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A composite negative electrode material, characterized in that: It comprises an inner core and a coating layer coated on the outer surface of the inner core, wherein the inner core is graphite and the coating layer is nano-diamond.
2. The composite negative electrode material according to claim 1, characterized in that: The graphite has a particle size D50 of 8-20 μm and a specific surface area of 0.8-4.0 m 2 / g, compacted density is 1.5-2.0cm 3 / g, gram capacity is greater than or equal to 335mAh / g.
3. The composite negative electrode material according to claim 1, characterized in that: The particle size D50 of the nano-diamond is 5-100 nm.
4. The composite negative electrode material according to claim 1, characterized in that The nanodiamond includes one or more of natural nanodiamond, nanodiamond modified by oxygen groups, nanodiamond modified by nitrogen groups, and nanodiamond modified by phosphorus groups.
5. A method for preparing a composite negative electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, dispersing nanodiamonds in a liquid coating agent to obtain a nanodiamond liquid coating agent; Step S2, mixing graphite with the nano-diamond liquid phase coating agent obtained in step S1 to obtain a precursor; Step S3, placing the precursor obtained in step S2 in an inert atmosphere for carbonization treatment, and cooling, to obtain the composite negative electrode material.
6. The method for preparing a composite negative electrode material according to claim 5, characterized in that: In step S1, the mass ratio of the nanodiamond to the liquid coating agent is 1:(20-100).
7. The method for preparing a composite negative electrode material according to claim 5, characterized in that: In step S1, the liquid coating agent is a mixture of one or more of heterocyclic aromatic hydrocarbons, ketones, hydrocarbons, resins, petroleum asphalt, and coal tar; the viscosity of the liquid coating agent is 20-100 mPa·s, and the residual carbon value is 5-40%.
8. The method for preparing a composite negative electrode material according to claim 5, characterized in that: In step S1, the dispersion method is ultrasonic dispersion, the ultrasonic frequency is 30-80 Hz, the power is 2000-3000 W, and the ultrasonic stirring time is 0.5-5 h.
9. The method for preparing a composite negative electrode material according to claim 5, characterized in that: In step S2, the mass ratio of the nano-diamond liquid phase coating agent to the graphite is (1-10):
100.
10. The method for preparing a composite negative electrode material according to claim 5, characterized in that: In step S3, the temperature of the carbonization treatment is 900-1200°C, the heating time is 9-15h, the heat preservation time is 5-8h, and the cooling time is 6-12h.
11. A negative electrode sheet, characterized in that: The composite negative electrode material comprises the composite negative electrode material according to any one of claims 1 to 4.
12. A lithium ion battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet according to claim 11.