Preparation method and application of modified carbon-coated lithium iron phosphate positive electrode material
By introducing boron/nitrogen co-doped single-wall carbon nanotubes and polyacrylate-polyacrylamide-polystyrene triblock copolymers into lithium iron phosphate batteries, the electrochemical performance of lithium iron phosphate batteries is solved. The poor problem improves the battery's conductivity efficiency and capacity.
Patent Information
- Application Number
- CN202411545695.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-01
AI Technical Summary
Due to the low electronic conductivity and lithium ion diffusion rate, lithium iron phosphate batteries have poor electrochemical performance, which limits their wide application in lithium-ion power batteries.
The preparation method of modified carbon-coated lithium iron phosphate positive electrode material is adopted, and the introduction of boron/nitrogen co-doped single-wall carbon nanotubes into the lithium iron phosphate precursor is formed to form a three-dimensional conductive network, which improves the electronic conductivity and lithium ion transmission speed. , and the polyacrylate-polyacrylamide-polystyrene triblock copolymer is used as a dispersant to prevent carbon nanotube agglomeration and enhance the carbon cladding structure.
The electrochemical performance and capacitance of lithium iron phosphate positive electrode material has been significantly improved, the conductivity efficiency and rate performance have been improved, the self-defects of lithium iron phosphate material have been compensated, and the overall performance of lithium ion batteries has been improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium iron phosphate batteries, and in particular relates to a preparation method of a modified carbon-coated lithium iron phosphate positive electrode material and an application thereof. Background Art
[0002] Lithium iron phosphate battery refers to a lithium-ion battery that uses lithium iron phosphate as the positive electrode material. Olivine-type lithium iron phosphate is currently the most promising positive electrode material for lithium-ion power batteries, with advantages such as a wide range of raw material sources, green and environmentally friendly, high theoretical specific capacity, good cycle performance and thermal stability. Among them, lithium iron phosphate contains a stable PO bond, which is difficult to decompose. Under high temperature or overcharge conditions, the structure of lithium iron phosphate will not collapse. Its operating voltage is stable and has an ultra-long cycle life, becoming a current research hotspot.
[0003] However, due to its inherent defects, lithium iron phosphate has very low electronic conductivity and lithium ion diffusion rate, which in turn leads to poor electrochemical performance of lithium iron phosphate, limiting its widespread application in lithium-ion power batteries. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a modified carbon-coated lithium iron phosphate positive electrode material and its application, so as to solve the problem of poor electrochemical performance of the lithium iron phosphate positive electrode material.
[0005] The purpose of the present invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a method for preparing a modified carbon-coated lithium iron phosphate positive electrode material, comprising the following process steps: S1. The lithium source, the iron source, the phosphorus source, the first carbon source, the cationic dopant and the first dispersant are uniformly mixed in a solvent to obtain a reaction premix; S2. After the reaction premix is ground and dried, the first sintering is performed under an inert gas atmosphere to obtain a lithium iron phosphate precursor; S3. The obtained lithium iron phosphate precursor, the second carbon source and the second dispersant are added to water, mixed evenly, wet ground, spray dried, and finally sintered for a second time under an inert gas atmosphere to obtain a modified carbon-coated lithium iron phosphate cathode material; The second carbon source is composed of an inorganic carbon source and an organic carbon source in a mass ratio of 1:(0.6-0.8); the inorganic carbon source is a boron / nitrogen co-doped single-walled carbon nanotube.
[0006] Preferably, the first carbon source comprises a combination of one or more of glucose, sucrose, starch, citric acid, amino acids, sodium acetate, polyethylene, polyethylene glycol and polyvinylidene fluoride; the organic carbon source comprises a combination of one or more of sucrose, polyvinyl alcohol, fructose, glucose, polyvinyl pyrrolidone, starch, citric acid, cyclodextrin and maltose.
[0007] Preferably, the molar ratio of the lithium source, the iron source and the phosphorus source is (0.90-1.20): (0.95-1.15): (0.90-1.20).
[0008] Preferably, the lithium source includes one or more combinations of lithium hydroxide, dilithium hydrogen phosphate, lithium nitrate, lithium dihydrogen phosphate, lithium monohydrogen phosphate, lithium carbonate, lithium oxalate, lithium chloride, lithium acetate and lithium phosphate.
[0009] Preferably, the iron source comprises a combination of one or more of ferrous oxalate, ferrous acetate, ferrous chloride, ferrous sulfate, ferric oxide, ferric phosphate, ferric nitrate, ferric chloride, ferric sulfate, ferric hydroxide, ferric carbonate, ferric citrate and ferric acetate.
[0010] Preferably, the phosphorus source includes one or more combinations of ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, iron phosphate, sodium phosphate, manganese phosphate, pyrophosphoric acid, lithium phosphate and lithium dihydrogen phosphate.
[0011] Preferably, the cationic dopant includes a combination of one or more of titanium dioxide, magnesium hydroxide, vanadium pentoxide, aluminum oxide, magnesium oxide, cobalt oxide, calcium oxide, calcium carbonate and niobium trioxide.
[0012] Preferably, the solvent includes deionized water, ethanol, or a combination of the two.
[0013] Preferably, the inert gas atmosphere includes one of a nitrogen atmosphere, an argon atmosphere, and a nitrogen-argon mixed atmosphere.
[0014] Preferably, the added amount of the first carbon source is 3-8% of the mass of the iron source.
[0015] Preferably, the amount of the cationic dopant added is 0.5-1% of the mass of the iron source.
[0016] Preferably, in the first sintering process, the sintering temperature is 400-800° C. and the sintering time is 2-8 hours.
[0017] Preferably, in the second sintering process, the sintering temperature is 700-800° C. and the sintering time is 4-8 hours.
[0018] By adopting the above technical solution, the lithium iron phosphate positive electrode material of the present invention is subjected to carbon coating treatment, and the carbon coating treatment can effectively improve the conductivity efficiency and improve the low conductivity of the lithium iron phosphate material. Furthermore, the present invention uses secondary sintering technology to increase the compaction density of the material while introducing carbon nanotubes as one of the carbon sources of the lithium iron phosphate positive electrode material.
[0019] The unique one-dimensional structure of single-walled carbon nanotubes can form an effective conductive network structure in the positive electrode material, accelerate the transmission speed of lithium ions, shorten the diffusion path of lithium ions, and greatly improve the electrochemical performance of lithium iron phosphate by accelerating the transfer speed of charge in the lithium iron phosphate positive electrode material. In addition, the hollow pipe structure of the carbon nanotube itself also enables it to have a certain ability to store lithium ions, which to a certain extent improves the capacity of lithium iron phosphate batteries and solves the problem of insufficient capacity of lithium iron phosphate batteries.
[0020] In addition, the single-walled carbon nanotubes of the present invention have also been subjected to boron / nitrogen co-doping modification treatment, and the nitrogen-boron bond length is similar to the carbon-carbon bond length, so the use of boron / nitrogen co-doped carbon nanotubes will not affect the structure of the carbon nanotubes themselves. In addition, compared with general nitrogen-doped carbon nanotubes, boron / nitrogen co-doped carbon nanotubes can better improve the conductivity and discharge specific capacity of the positive electrode material. Nitrogen atom doping can provide more electron donors, increase the free carriers in the material, and improve the electronic conductivity of the material. Boron atom doping can provide more electron acceptors. Nitrogen atoms and boron atoms cooperate with each other, which can promote the migration of electrons from the lithium iron phosphate material to the surface during the charging process, and also facilitate the migration of electrons from the carbon coating layer back to the lithium iron phosphate material during the discharge process, thereby improving the conductive efficiency of the material, giving the lithium iron phosphate positive electrode material excellent electrochemical properties, and making up for the defects of the lithium iron phosphate material itself.
[0021] Preferably, the mass ratio of the second carbon source to the lithium iron phosphate precursor is (0.06-0.12):1.
[0022] Preferably, the raw material of the boron / nitrogen co-doped single-walled carbon nanotubes comprises single-walled carbon nanotubes, a nitrogen source and a boron source in a mass ratio of 1:(1.5-2):(0.2-0.3).
[0023] Preferably, the nitrogen source includes one or more of urea, melamine and dicyandiamide; and the boron source is triphenylborate.
[0024] By adopting the above technical scheme, the present invention further modifies single-walled carbon nanotubes by co-doping with boron / nitrogen. The carbon nanotubes after doping form a new three-dimensional conductive network on the surface of the lithium iron phosphate positive electrode material. The internal interlaced carbon nanotube pore structure can provide a channel for rapid transmission of electrons and lithium ions, improve electronic conductivity, shorten the diffusion distance of lithium ions, and improve the electrochemical performance of the positive electrode material. In addition, the unique electronic structure of boron / nitrogen can change the charge distribution of carbon nanotubes and carbon coatings, which is conducive to the formation of uniform carbon nanoparticles adsorbed on the surface of the positive electrode material, and improve the conductivity and discharge specific capacity of the positive electrode material. In particular, the addition of boron atoms can also increase the defect edge by changing the charge density of adjacent carbon atoms to activate the inert carbon skeleton, thereby improving the activity of carbon nanotubes and the transmission speed of lithium ions.
[0025] Furthermore, the boron / nitrogen co-doped single-walled carbon nanotubes of the present invention are used as the second carbon source, and are compounded with the lithium iron phosphate positive electrode material through the second sintering treatment. The lithium iron phosphate precursor obtained after the first sintering has a smaller impedance, which is conducive to the dispersion of the boron / nitrogen co-doped single-walled carbon nanotubes between the lithium iron phosphate particles. After the second sintering, they can be evenly dispersed in the lithium iron phosphate positive electrode material, providing more lithium ion transmission channels. In addition, the resistance of the lithium iron phosphate positive electrode material after the second sintering is smaller, and the hindrance to the diffusion of lithium ions is reduced, which can further improve the rate performance of the lithium iron phosphate positive electrode material and improve the electrochemical performance of the lithium iron phosphate positive electrode material.
[0026] Preferably, the boron / nitrogen co-doped single-walled carbon nanotubes are prepared according to the following method: Pretreatment of carbon nanotubes: disperse single-walled carbon nanotubes in a strong acid solution, raise the temperature to 30-40°C, stir and disperse for 3-4 hours, and obtain pretreated single-walled carbon nanotubes by filtering, washing and drying; Preparation of boron / nitrogen co-doped carbon nanotubes: Pretreated single-walled carbon nanotubes, nitrogen source and boron source are placed in the same crucible, and vapor deposition is performed in a nitrogen atmosphere to obtain boron / nitrogen co-doped single-walled carbon nanotubes, wherein the vapor deposition temperature is 950-1000°C.
[0027] Preferably, the strong acid solution includes one or a combination of concentrated sulfuric acid and concentrated nitric acid.
[0028] By adopting the above technical solution, the number of oxygen-containing functional groups on the surface of the single-walled carbon nanotube increases after pretreatment, which is conducive to the doping and bonding of heteroatoms and improving the dispersibility of the carbon nanotube during the preparation process. The present invention adopts a vapor deposition method to dope and modify the carbon nanotube. The vapor deposition can make nitrogen atoms and boron atoms evenly distributed and deposited in the carbon nanotube, so that the synergistic effect between nitrogen atoms and boron atoms can be better exerted, and the conductivity and specific capacity of the doped and modified carbon nanotube can be improved.
[0029] Preferably, the first dispersant includes a combination of one or more of citric acid, succinic acid, tripropyl phosphate, dibutyl phosphate, polyamide-based silicone oil, methylcyclosiloxane, sodium dodecylbenzene sulfonate and sodium octylbenzene sulfonate; the second dispersant is a polyacrylate-polyacrylamide-polystyrene triblock copolymer.
[0030] Preferably, the amount of the first dispersant added is 2-4% of the mass of the iron source.
[0031] Preferably, the mass ratio of the second dispersant to the lithium iron phosphate precursor is (0.02-0.04):1.
[0032] By adopting the above technical solution, boron / nitrogen co-doped single-walled carbon nanotubes can provide a large number of transmission channels for electrons and lithium ions in lithium iron phosphate positive electrode materials, improve transmission efficiency and shorten diffusion paths, and change the surface charge distribution of carbon nanotubes through doping modification, improve the conductivity and specific capacity of the material, and thus improve the electrochemical performance of the material. However, carbon nanotubes are prone to agglomeration, and after agglomeration, carbon nanotubes cannot form an effective conductive network structure on the surface of the positive electrode material, which in turn affects the electrochemical properties of the positive electrode material.
[0033] Therefore, the present invention adds a second dispersant while adding carbon nanotubes. Compared with general dispersants, the polyacrylate-polyacrylamide-polystyrene triblock copolymer will not introduce other metal ions or impurity molecules during the second sintering process, thereby affecting the improvement of the charge distribution of the carbon nanotubes by boron / nitrogen in the boron / nitrogen co-doped single-walled carbon nanotubes, and affecting the interface stability of the positive electrode material. The amino polar functional groups contained in the polyacrylate-polyacrylamide-polystyrene triblock copolymer can interact with the polar groups on the surface of the carbon nanotubes and adsorb on the surface of the carbon nanotubes. At the same time, the molecular structure of the block copolymer can form a three-dimensional barrier in the dispersion medium, thereby preventing the agglomeration between the carbon nanotubes, achieving uniform dispersion of the carbon nanotubes between the lithium iron phosphate particles, and achieving the formation of a conductive three-dimensional network, thereby improving the electrochemical performance of the positive electrode material.
[0034] Preferably, the polyacrylate-polyacrylamide-polystyrene triblock copolymer is prepared according to the following method: an emulsifier is dissolved in deionized water and then an acrylic acid monomer is added, the mixture is stirred and mixed in an ice water bath for 30 to 40 minutes, an initiator and a catalyst are added, the temperature is raised to 35 to 45° C. in a nitrogen atmosphere, the mixture is stirred and reacted for 1 to 2 hours, acrylamide and a catalyst are then added, the reaction is continued with stirring for 1 to 2 hours, and finally styrene and a catalyst are added, and the mixture is reacted for 5 to 6 hours to obtain a polyacrylate-polyacrylamide-polystyrene triblock copolymer.
[0035] Preferably, the emulsifier includes a combination of one or more of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate.
[0036] Preferably, the initiator includes one or more of iodoform, azobisisobutyronitrile and ammonium persulfate.
[0037] Preferably, the catalyst comprises one or a combination of sodium bicarbonate and sodium dithionite.
[0038] Preferably, the acrylic monomer includes one or more of methyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, methyl methacrylate, glycidyl acrylate, and methacrylic acid.
[0039] Preferably, the mass ratio of acrylic acid monomer, acrylamide and styrene is 1:(0.4-0.8):(0.5-1).
[0040] By adopting the above technical scheme, the polyacrylate-polyacrylamide-polystyrene triblock copolymer obtained by the present invention, acrylamide is used to introduce amino groups into the molecular chain of the polyacrylate-polyacrylamide-polystyrene triblock copolymer, polyacrylate is the main skeleton structure, and polystyrene has strong rigidity. In addition to being able to promote the formation of a three-dimensional barrier, it can also be coated on the surface of a lithium iron phosphate positive electrode material after secondary sintering, thereby enhancing the carbon layer structure, compensating for the defects of the carbon layer, and making the carbon coating layer uniformly and smoothly coated on the surface of the positive electrode material. At the same time, the interaction between the positive electrode material and the electrolyte is coordinated, and the embedding and extraction activity of lithium ions during the charge and discharge process is enhanced, so that the raw material has good reaction activity and uniform physical and chemical properties, thereby improving the conductivity of the positive electrode material.
[0041] In a second aspect, the present invention provides an application of a modified carbon-coated lithium iron phosphate positive electrode material in a lithium-ion battery positive electrode material.
[0042] Beneficial effects of the present invention: 1. The present invention introduces boron / nitrogen co-doped single-walled carbon nanotubes as an inorganic carbon source for the material during the process of carbon-coating lithium iron phosphate. The unique pore structure of the carbon nanotubes themselves can accelerate the transmission speed of lithium ions, shorten the diffusion path of lithium ions, and thus improve the electrochemical performance and capacity of lithium iron phosphate. The single-walled carbon nanotubes modified by boron / nitrogen co-doping can form a new three-dimensional conductive network on the surface of the lithium iron phosphate positive electrode material, improve the electronic conductivity, and the nitrogen atoms and boron atoms can cooperate with each other, by changing the charge distribution of the carbon nanotubes and the carbon coating layer, the conductivity of the carbon coating layer is enhanced, thereby improving the conductive efficiency of the material, and giving the lithium iron phosphate positive electrode material excellent electrochemical properties.
[0043] 2. The raw materials of the lithium iron phosphate positive electrode material of the present invention also include polyacrylate-polyacrylamide-polystyrene triblock copolymer as a dispersant for boron / nitrogen co-doped single-walled carbon nanotubes. The amino groups contained therein can interact with the polar groups on the surface of the carbon nanotubes and adsorb on the surface of the carbon nanotubes. At the same time, the molecular structure of the block copolymer can form a three-dimensional barrier in the dispersion medium to prevent the agglomeration of carbon nanotubes and reduce the adverse effects caused by agglomeration. In addition, the introduction of polyacrylate-polyacrylamide-polystyrene triblock copolymer can also enhance the structure of the carbon coating layer, make up for the defects of the carbon coating layer, and improve the electrochemical performance and specific capacity of the positive electrode material. DETAILED DESCRIPTION
[0044] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Preparation Example Preparation Example 1 Boron / Nitrogen Co-doped Single-walled Carbon Nanotubes Preparation Example 1-1, a boron / nitrogen co-doped single-walled carbon nanotube, prepared according to the following method: Pretreatment of carbon nanotubes: 10 g of single-walled carbon nanotubes (diameter 1-2 nm, length 5-30 μm) were dispersed in 250 mL of concentrated nitric acid solution, the temperature was raised to 35°C, stirred and dispersed for 4 h, and the pretreated single-walled carbon nanotubes were obtained by filtration, washing and drying; Preparation of boron / nitrogen co-doped carbon nanotubes: 10 g of pretreated single-walled carbon nanotubes, 18 g of urea and 2.5 g of triphenylborate were placed in the same crucible and vapor deposited in a nitrogen atmosphere to obtain boron / nitrogen co-doped single-walled carbon nanotubes, wherein the vapor deposition temperature was 980°C.
[0046] Preparation Example 1-2, a boron / nitrogen co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that the amount of urea added is 15 g, and the amount of triphenylborate added is 2.5 g.
[0047] Preparation Example 1-3, a boron / nitrogen co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that the amount of urea added is 20 g and the amount of triphenylborate added is 3 g.
[0048] Preparation Example 1-4, a boron / nitrogen co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that the amount of triphenylborate added is 1.5 g.
[0049] Preparation Example 1-5, a boron / nitrogen co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that the amount of triphenylborate added is 3.5 g.
[0050] Preparation Example 1-6, a nitrogen co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that triphenylborate is not added.
[0051] Preparation Example 1-7, a boron co-doped single-walled carbon nanotube, is different from Preparation Example 1-1 only in that urea is not added.
[0052] Preparation Example 2 Polyacrylate-polyacrylamide-polystyrene triblock copolymer Preparation Example 2-1, a polyacrylate-polyacrylamide-polystyrene triblock copolymer, prepared according to the following method: 1 g of sodium dodecyl sulfate was dissolved in 500 mL of deionized water, and then 10 g of butyl acrylate was added. The mixture was stirred in an ice-water bath for 30 min, and 0.5 g of iodoform and 0.2 g of sodium bicarbonate were added. The temperature was raised to 40° C. under a nitrogen atmosphere, and the mixture was stirred for 1 h. Subsequently, 6 g of acrylamide and 0.1 g of sodium bicarbonate were added, and the stirring reaction was continued for 1 h. Finally, 8 g of styrene and 0.2 g of sodium bicarbonate were added, and the mixture was reacted for 6 h to obtain a polyacrylate-polyacrylamide-polystyrene triblock copolymer.
[0053] Preparation Example 2-2, a polyacrylate-polyacrylamide-polystyrene triblock copolymer, is different from Preparation Example 2-1 only in that the amount of acrylamide added is 4 g and the amount of styrene added is 10 g.
[0054] Preparation Example 2-3, a polyacrylate-polyacrylamide-polystyrene triblock copolymer, is different from Preparation Example 2-1 only in that the amount of acrylamide added is 8 g and the amount of styrene added is 5 g.
[0055] Preparation Example 2-4, a polyacrylate-polyacrylamide block copolymer, was prepared according to the following method: 1 g of sodium dodecyl sulfate was dissolved in 500 mL of deionized water, and 10 g of butyl acrylate was added. The mixture was stirred in an ice-water bath for 30 min. 0.5 g of iodoform and 0.2 g of sodium bicarbonate were added. The temperature was raised to 40° C. under a nitrogen atmosphere, and the mixture was stirred for 1 h. Subsequently, 6 g of acrylamide and 0.1 g of sodium bicarbonate were added, and the mixture was stirred for 3 h to obtain a polyacrylate-polyacrylamide block copolymer.
[0056] Preparation Example 2-5, a polyacrylate-polystyrene block copolymer, was prepared according to the following method: 1 g of sodium dodecyl sulfate was dissolved in 500 mL of deionized water, and 10 g of butyl acrylate was added. The mixture was stirred for 30 min in an ice-water bath. 0.5 g of iodoform and 0.2 g of sodium bicarbonate were added. The temperature was raised to 40° C. under a nitrogen atmosphere, and the mixture was stirred for 2 h. Subsequently, 8 g of styrene and 0.2 g of sodium bicarbonate were added. After reacting for 6 h, a polyacrylate-polystyrene block copolymer was obtained.
[0057] Preparation Example 2-6, a polyacrylate, prepared according to the following method: 1 g of sodium dodecyl sulfate was dissolved in 500 mL of deionized water, and then 10 g of butyl acrylate was added. The mixture was stirred for 30 min in an ice-water bath. 0.5 g of iodoform and 0.2 g of sodium bicarbonate were added. The temperature was raised to 40° C. under a nitrogen atmosphere, and the mixture was stirred for 4 h to obtain polyacrylate.
[0058] Example Example 1, a modified carbon-coated lithium iron phosphate positive electrode material is prepared by the following process steps: S1. 11 g of lithium dihydrogen phosphate, 40 g of ferric sulfate, 15.7 g of ammonium phosphate, 2.4 g of citric acid, 0.32 g of vanadium pentoxide and 1.2 g of tripropyl phosphate were mixed in 250 mL of a 25% ethanol aqueous solution to obtain a reaction premix; S2. After the reaction premix is ground and dried, the first sintering is performed under a nitrogen gas atmosphere to obtain a lithium iron phosphate precursor, wherein the sintering temperature of the first sintering is 550° C. and the sintering time is 6 h; S3. Add 50g of the obtained lithium iron phosphate precursor, 4.5g of the second carbon source and 1.5g of the polyacrylate-polyacrylamide-polystyrene triblock copolymer obtained in Preparation Example 2-1 into 500mL of water, mix well, perform wet grinding, spray drying, and finally perform a second sintering under a nitrogen gas atmosphere, wherein the second sintering temperature is 750°C and the sintering time is 6h, and finally obtain a modified carbon-coated lithium iron phosphate positive electrode material.
[0059] The second carbon source is a mixture of the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 and β-cyclodextrin (purity ≥ 98%) in a mass ratio of 1:0.7.
[0060] Embodiments 2 to 5 are modified carbon-coated lithium iron phosphate positive electrode materials, which differ from Embodiment 1 only in that the raw materials and the ratio of the raw materials are adjusted, as shown in Table 1:
[0061] Among them, the second carbon source in Example 2 is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-1 with a mass ratio of 1:0.6; the second carbon source in Example 3 is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-1 with a mass ratio of 1:0.8; the second carbon source in Example 4 is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-2 with a mass ratio of 1:0.7; the second carbon source in Example 5 is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-3 with a mass ratio of 1:0.7.
[0062] The polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-2 was used in Example 2; the polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-3 was used in Example 3; the polyacrylate-polyacrylamide-polystyrene triblock copolymer used in Examples 4 and 5 was the same as that in Example 1.
[0063] Example 6, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 are replaced with an equal amount of boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-4.
[0064] Example 7, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 are replaced with an equal amount of boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-5.
[0065] Example 8, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that the polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-1 is replaced by an equal amount of the polyacrylate-polyacrylamide block copolymer prepared in Preparation Example 2-4.
[0066] Example 9, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that the polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-1 is replaced by an equal amount of the polyacrylate-polystyrene block copolymer prepared in Preparation Example 2-5.
[0067] Comparative Example Comparative Example 1, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the second carbon source is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-1 in a mass ratio of 1:1.
[0068] Comparative Example 2, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the second carbon source is a mixture of boron / nitrogen co-doped single-walled carbon nanotubes and β-cyclodextrin prepared in Preparation Example 1-1 in a mass ratio of 1:0.4.
[0069] Comparative Example 3, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 are replaced with an equal amount of nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-6.
[0070] Comparative Example 4, a modified carbon-coated lithium iron phosphate positive electrode material, differs from Example 1 only in that the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 are replaced with an equal amount of boron co-doped single-walled carbon nanotubes prepared in Preparation Example 1-7.
[0071] Comparative Example 5, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that the boron / nitrogen co-doped single-walled carbon nanotubes prepared in Preparation Example 1-1 are replaced by an equal amount of single-walled carbon nanotubes.
[0072] Comparative Example 6, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that the second carbon source is β-cyclodextrin.
[0073] Comparative Example 7, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that the polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-1 is replaced by an equal amount of the polyacrylate prepared in Preparation Example 2-6.
[0074] Comparative Example 8, a modified carbon-coated lithium iron phosphate positive electrode material, is different from Example 1 only in that an equal amount of tripropyl phosphate is used to replace the polyacrylate-polyacrylamide-polystyrene triblock copolymer prepared in Preparation Example 2-1.
[0075] Performance testing The lithium iron phosphate cathode materials obtained in the examples and comparative examples were assembled into 2032-type button cells for electrochemical performance testing, wherein the metal lithium sheet was used as the negative electrode and reference electrode, the polypropylene microporous membrane was used as the separator, and LIPF6 / EC+DMC was used as the electrolyte. The discharge specific capacity (mAh / g) of the lithium battery obtained by the test at different rates (0.1C, 1C and 10C) was measured, wherein the test temperature was 25°C and the test voltage range was 2.0-3.8V.
[0076] The above test results are shown in Table 2:
[0077] According to Table 2, in combination with Example 1 and Example 2 to Example 5, it can be seen that there is no significant difference in the discharge specific capacity at different rates between Example 2 to Example 5 and Example 1. The difference between Example 2 to Example 5 and Example 1 is only that the raw materials and the raw material ratio are adjusted within the required range, which has little effect on the electrochemical performance of the obtained positive electrode material.
[0078] Combining Example 1, Example 6 and Example 7, it can be seen that the discharge specific capacity of Example 6 and Example 7 is reduced compared with that of Example 1, and the decay rate of the discharge capacity increases with the increase of the rate. Example 6 and Example 7 change the doping amount of boron atoms in the boron / nitrogen co-doped single-walled carbon nanotubes. Specifically, Example 6 reduces the doping amount of boron, the electron acceptor provided by boron atoms to the positive electrode material is reduced, the effect of improving the charge distribution on the surface is reduced, and the synergistic effect with nitrogen atoms is reduced, so the electrochemical performance of the positive electrode material is reduced; Example 7 increases the doping amount of boron. A large amount of boron atoms doping will destroy the electronic structure of the single-walled carbon nanotubes, thereby affecting the specific capacity of the positive electrode material.
[0079] Combining Example 1, Example 8, Example 9, Comparative Example 7 and Comparative Example 8, it can be seen that the discharge specific capacity of Example 8, Example 9, Comparative Example 7 and Comparative Example 8 is reduced compared with that of Example 1, and with the increase of the rate, the decay rate of the discharge capacity is significantly increased. Compared with Example 1, Example 8, Example 9, Comparative Example 7 and Comparative Example 8 change the composition of the second dispersant polyacrylate-polyacrylamide-polystyrene triblock copolymer. Specifically, Example 8 does not contain a polystyrene block, which will not only affect the formation of a steric barrier to a certain extent, but also reduce the reinforcing effect of the polyacrylate-polyacrylamide-polystyrene triblock copolymer on the carbon coating layer, increase the defects of the carbon coating layer, and cause the electrochemical performance of the obtained positive electrode material to decrease; Example 9 does not contain a polyacrylamide block, lacks the effect of the amino polar group, and the dispersing effect of the polyacrylate-polyacrylamide-polystyrene triblock copolymer on the carbon nanotubes is greatly reduced, resulting in the carbon nanotubes being easily agglomerated during the preparation process, thereby affecting the electrochemical performance of the positive electrode material. Comparative Example 7 does not have a polystyrene block and a polyacrylamide block, the dispersion effect is significantly reduced, and the electrochemical performance of the material is reduced. In Comparative Example 8, conventional dispersants are used, which have certain dispersing effects but are inferior to polyacrylate-polyacrylamide-polystyrene triblock copolymers, and cannot adjust the interaction between the positive electrode material and the electrolyte, thereby enhancing the reversible electrochemical reaction of the lithium battery.
[0080] Combining Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the discharge specific capacity of Comparative Example 1 and Comparative Example 2 is reduced compared with that of Example 1. In Comparative Example 1, the amount of carbon nanotubes added was reduced, the conductive network density on the surface of the positive electrode material decreased, the conductive performance decreased, and the transmission rate and diffusion rate of lithium ions were reduced, thereby affecting the electrochemical performance of the positive electrode material. In Comparative Example 2, the amount of carbon nanotubes added was increased, and the carbon nanotubes were too much, and they were easy to agglomerate, which was not conducive to the increase of the electrochemical performance of the positive electrode material.
[0081] Combined with Example 1 and Comparative Examples 3 to 6, it can be seen that the discharge specific capacity of Comparative Examples 3 to 6 is significantly reduced compared with that of Example 1, and the decay rate of the discharge capacity is significantly increased with the increase of the rate. In Comparative Example 3, the carbon nanotubes are not doped with boron atoms. On the one hand, there is a lack of improvement in the charge distribution of the carbon coating layer by boron atoms, and on the other hand, the content of the electron acceptor of the material decreases, making it difficult to coordinate with nitrogen atoms; in Comparative Example 4, there is no doping with nitrogen atoms, the content of carriers in the material decreases, the conductivity of the positive electrode material decreases, and the conductivity of the conductive network formed decreases, thereby affecting the electrochemical properties of the positive electrode material; in Comparative Example 5, the carbon nanotubes are not doped and modified, and the performance decreases more significantly; in Comparative Example 6, no carbon nanotubes are added, and there is a lack of a conductive network formed by carbon nanotubes on the surface of the positive electrode material, the transmission speed of lithium ions decreases, the diffusion distance increases, and the conductivity and discharge specific capacity of the positive electrode material decrease significantly.
[0082] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a modified carbon-coated lithium iron phosphate positive electrode material, It is characterized in that The process steps include: S1. The lithium source, the iron source, the phosphorus source, the first carbon source, the cationic dopant and the first dispersant are uniformly mixed in a solvent to obtain a reaction premix; S2. After the reaction premix is ground and dried, the first sintering is performed under an inert gas atmosphere to obtain a lithium iron phosphate precursor; S3. The obtained lithium iron phosphate precursor, the second carbon source and the second dispersant are added to water, mixed evenly, wet ground, spray dried, and finally sintered for a second time under an inert gas atmosphere to obtain a modified carbon-coated lithium iron phosphate cathode material; The second carbon source is composed of an inorganic carbon source and an organic carbon source in a mass ratio of 1:(0.6-0.8); the inorganic carbon source is a boron / nitrogen co-doped single-walled carbon nanotube; The second dispersant is a polyacrylate-polyacrylamide-polystyrene triblock copolymer; The polyacrylate-polyacrylamide-polystyrene triblock copolymer is prepared according to the following method: an emulsifier is dissolved in deionized water and then an acrylic acid monomer is added, the mixture is stirred and mixed in an ice water bath for 30 to 40 minutes, an initiator and a catalyst are added, the temperature is raised to 35 to 45° C. in a nitrogen atmosphere, the mixture is stirred and reacted for 1 to 2 hours, acrylamide and a catalyst are subsequently added, the mixture is stirred and reacted for 1 to 2 hours, styrene and a catalyst are finally added, and the mixture is reacted for 5 to 6 hours to obtain the polyacrylate-polyacrylamide-polystyrene triblock copolymer.
2. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 1, It is characterized in that The mass ratio of the second carbon source to the lithium iron phosphate precursor is (0.06-0.12):
1.
3. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 1, It is characterized in that The raw materials of the boron / nitrogen co-doped single-walled carbon nanotubes include single-walled carbon nanotubes, a nitrogen source and a boron source in a mass ratio of 1:(1.5-2):(0.2-0.3).
4. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 3, It is characterized in that The nitrogen source includes one or more of urea, melamine and dicyandiamide; and the boron source is triphenylborate.
5. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 3, It is characterized in that The boron / nitrogen co-doped single-walled carbon nanotubes are prepared according to the following method: Pretreatment of carbon nanotubes: disperse single-walled carbon nanotubes in a strong acid solution, raise the temperature to 30-40°C, stir and disperse for 3-4 hours, and obtain pretreated single-walled carbon nanotubes by filtering, washing and drying; Preparation of boron / nitrogen co-doped carbon nanotubes: Pretreated single-walled carbon nanotubes, nitrogen source and boron source are placed in the same crucible, and vapor deposition is performed in a nitrogen atmosphere to obtain boron / nitrogen co-doped single-walled carbon nanotubes, wherein the vapor deposition temperature is 950-1000°C.
6. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 1, It is characterized in that The first carbon source includes a combination of one or more of glucose, sucrose, starch, citric acid, amino acids, sodium acetate, polyethylene, polyethylene glycol and polyvinylidene fluoride; the organic carbon source includes a combination of one or more of sucrose, polyvinyl alcohol, fructose, glucose, polyvinyl pyrrolidone, starch, citric acid, cyclodextrin and maltose.
7. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 1, It is characterized in that The first dispersant includes a combination of one or more of citric acid, succinic acid, tripropyl phosphate, dibutyl phosphate, polyamide-based silicone oil, methylcyclosiloxane, sodium dodecylbenzene sulfonate and sodium octylbenzene sulfonate.
8. The method for preparing the modified carbon-coated lithium iron phosphate positive electrode material according to claim 1, It is characterized in that The molar ratio of the lithium source, the iron source and the phosphorus source is (0.90-1.20): (0.95-1.15): (0.90-1.20).
9. Use of the modified carbon-coated lithium iron phosphate positive electrode material prepared by the preparation method according to any one of claims 1 to 8 in positive electrode materials for lithium-ion batteries.
Citation Information
Patent Citations
Method and device for producing carbon nano-tube or nitrogen doping carbon nano-tube with liquid phase forerunner article
CN101244815A
Dispersion comprising carbon nanotubes and graphene platelets
CN103733271A
Preparation method for nitrogen-boron-doped carbon-based catalyst
CN104998675A
Nitrogen-doped carbon modified lithium iron phosphate positive electrode material
CN115133010A
Lithium iron phosphate positive electrode material, preparation method thereof and lithium ion battery positive electrode plate
CN115196612A
Cited By
Iron-based mixed phosphate positive electrode material, preparation method thereof and application of iron-based mixed phosphate positive electrode material and sodium battery
CN120637464A
Iron-based mixed phosphate cathode material, preparation method thereof, and application in sodium batteries