Battery positive electrode material as well as preparation method and application thereof

By doping nitrogen elements through ball milling and using carbon amide and conductive carbon black to modify manganese dioxide materials, the application problem of aqueous zinc-manganese batteries is solved, the discharge capacity and cycle stability of the battery are improved, and it is suitable for industrial production.

CN118738366APending Publication Date: 2024-10-01CHENGDU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410769678.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The application of aqueous zinc-manganese batteries is restricted by problems such as cathode dissolution, electrostatic interaction, zinc dendrites, corrosion, passivation and by-products, resulting in problems such as capacity fading, low Coulombic efficiency and short circuit, which limits its commercial development.

Method used

The ball milling method is used to dope nitrogen, and the manganese dioxide material is modified to enhance its conductivity and cycle stability. Carbon amide and conductive carbon black are used in the preparation process to reduce costs and energy consumption and improve the discharge of zinc-manganese batteries. ability.

Benefits of technology

It significantly improves the discharge capacity and cycle stability of zinc-manganese batteries, reduces preparation costs, is suitable for industrial production, and optimizes the charge transfer dynamics and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738366A_ABST
    Figure CN118738366A_ABST
Patent Text Reader

Abstract

The invention discloses a battery positive electrode material and a preparation method and application thereof, and belongs to the technical field of batteries. According to the prepared battery positive electrode material, the nitrogen element and the carbon element are doped into the manganese dioxide, oxygen vacancies with the proportion higher than that of the manganese dioxide and more active sites are provided, and the stability and the discharging capacity of an aqueous zinc-manganese battery can be improved; the preparation method provided by the invention is doping by a ball-milling method, and is beneficial to more simply and conveniently synthesizing a relatively ideal positive electrode material, so that the cycle and discharge performance of the battery is optimized, and the preparation process is simple, low in energy consumption, low in cost, small in environmental pollution and suitable for industrial requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery technology, and specifically relates to a battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Compared with lithium batteries and sodium batteries with various organic electrolytes, the high safety of rechargeable aqueous batteries makes them more popular in the field of large-scale energy storage. In recent years, a lot of research has been done on positive electrode materials, which can be simply divided into three main types, including vanadium-based positive electrodes, manganese-based cathodes, and Prussian blue analogs.

[0003] Among them, high energy density, cheap and pollution-free aqueous rechargeable zinc-manganese (Zn-Mn) batteries are considered to be one of the most promising aqueous battery systems, which has aroused the research interest of many researchers. In recent years, a large number of papers have reported the latest research results on Zn-Mn batteries, from improving the electrochemical performance of the positive electrode, optimizing the electrolyte to improving the reversibility of the metal zinc negative electrode. However, when aiming at large-scale commercial batteries, the application of Zn-Mn batteries still has obvious shortcomings.

[0004] Problems such as positive electrode dissolution, adverse effects of electrostatic interactions, zinc dendrites, corrosion, passivation and by-products may lead to capacity decay, low Coulombic efficiency and short circuit of aqueous zinc-manganese batteries, which seriously restricts the development and commercialization of aqueous zinc-manganese batteries. Summary of the invention

[0005] In view of the above-mentioned prior art, the present invention provides a battery positive electrode material and a preparation method and application thereof, which effectively solves the problems of complex doping process, high cost and high energy consumption of battery positive electrode materials in the prior art.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a positive electrode material for a battery, comprising the following steps:

[0007] S1: Manganese dioxide and a nitrogen source are mixed in a mass ratio of 7-9:1-3 to form a mixture 1, the mixture 1 is ball-milled at a speed of 300-500 r / min for 24h-48h, and the ball-milled mixture 1 is washed and dried at 100-200° C. for 8h-12h to obtain a crude product;

[0008] S2: The crude product and the carbon source are combined into a mixed material 2 in a mass ratio of 8 to 12:1, and the mixed material 2 is ball-milled at a speed of 300 to 500 r / min for 24 to 48 hours. The ball-milled mixed material 2 is then washed and dried at 50 to 100° C. for 16 to 24 hours to obtain the mixed material 2.

[0009] The beneficial effects of the present invention are as follows: the present invention adopts the strategy of ball milling to dope nitrogen element to synthesize stable cycle and discharge materials, and the MnO 2 The modified zinc-manganese battery H was made by doping nitrogen to change its crystal structure, enhance the conductivity of manganese dioxide raw materials, and change the cycle stability and discharge capacity of manganese dioxide raw materials when assembling batteries. + The ion diffusion behavior is improved, and finally the discharge capacity of the zinc-manganese battery is greatly improved; and the preparation process of the present invention is simple, low in energy consumption, low in cost, and low in environmental pollution, and is suitable for industrial needs.

[0010] Based on the above technical solution, the present invention can also be improved as follows.

[0011] Furthermore, the nitrogen source is carbon amide, and the carbon source is conductive carbon black.

[0012] The beneficial effects of adopting a further technical solution are: using carbon amide as a nitrogen source, which is low in cost and contains a high content of nitrogen, helps to more easily synthesize a more ideal positive electrode material, thereby optimizing the battery's cycle and discharge performance; and adding conductive carbon black to the positive electrode material can improve the material's conductivity.

[0013] Furthermore, in S1, water with a mass of 5 times that of manganese dioxide was used as the medium for ball milling, a ball-to-material ratio of 8:1, a rotation speed of 360 r / min, a ball milling time of 28 h, a drying temperature of 150° C., and a drying time of 10 h.

[0014] Furthermore, the ball mill in S2 uses water of 5 times the mass of the crude product as the medium, the ball-to-material ratio is 8:1, the rotation speed is 400 r / min, the ball milling time is 36 h, the drying temperature is 70° C., and the drying time is 20 h.

[0015] The beneficial effect of adopting a further technical solution is that a suitable rotation speed helps to provide sufficient energy, allowing the steel balls to exert high-energy impact and grinding on the manganese dioxide, breaking the crystal structure of the manganese dioxide, increasing the surface energy, thereby promoting phase change and the doping of atoms or molecules in the material.

[0016] The invention also discloses a method for preparing the battery positive electrode material to prepare the battery positive electrode material.

[0017] The beneficial effects of the present invention are as follows: the battery positive electrode material provided by the present invention has the characteristics of dense distribution, which helps to improve the stability of the battery during long cycles, has faster charge transfer kinetics and higher discharge capacity; and uses carbonamide as a doping nitrogen source to replace traditional precious metal doping, which significantly reduces the doping cost and is suitable for industrial needs.

[0018] The invention also discloses the application of the battery positive electrode material in the preparation of the zinc-manganese battery.

[0019] Furthermore, the battery positive electrode material, graphene and binder are mixed in a mass ratio of 7:2:1 to form a mixture three, and then a solvent is added and ground for 5 minutes to obtain a mixed slurry. The mixed slurry is coated on carbon paper and dried at 60°C and then cooled to room temperature to obtain a battery positive electrode; the material-liquid ratio of the mixture three to the solvent is 5g:1mL.

[0020] S2: The zinc sheet is used as the negative electrode and the glass fiber is used as the separator. The prepared battery positive electrode is placed in the battery shell, and the electrolyte is added. After sealing, the zinc-manganese battery is assembled; the electrolyte composition is ZnSO 4 With MnSO 4 , ZnSO 4 With MnSO 4 The molar ratio is 10:1.

[0021] Furthermore, the binder of S1 is polyvinylidene fluoride, and the solvent is N-methylpyrrolidone.

[0022] The beneficial effects of the present invention are as follows: a battery assembled using the battery positive electrode material provided by the present invention has excellent discharge performance and cycle stability; and the assembly material cost is low, and large-scale production is easy, which is suitable for industrialization needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 MnO prepared in Examples 1 to 4 2 (25% N), MnO 2 (10%N), MnO 2 (20%N), MnO 2 XRD characterization diagram of (30% N) and comparative example;

[0024] Figure 2 The MnO prepared in Example 1 2 (25% N), MnO 2 XRD characterization diagram of (25% NC) and comparative example;

[0025] Figure 3 TEM image of the comparative example at a size of 100 nm;

[0026] Figure 4 TEM image of the comparative example at a size of 200 nm;

[0027] Figure 5 The MnO prepared in Example 1 2 TEM image of (25% NC) at 100 nm size;

[0028] Figure 6 The MnO prepared in Example 1 2TEM image of (25% NC) at 200 nm size;

[0029] Figure 7 The MnO prepared in Example 1 2 SEM images of (25% NC) at 2 μm and 500 nm sizes;

[0030] Figure 8 The MnO prepared in Example 1 2 EDS mapping of (25% NC);

[0031] Fig. 9 is the state density diagram of the comparative example;

[0032] Fig.10 The MnO prepared in Example 1 2 Density of states diagram of (25% NC);

[0033] Fig.11 MnO prepared in Examples 1 to 4 2 (25% N), MnO 2 (10%N), MnO 2 (20%N), MnO 2 Long cycle voltammetry curves of zinc-manganese batteries assembled with positive electrode materials (30% N) and comparative examples;

[0034] Fig.12 The MnO prepared in Example 1 2 (25% N), MnO 2 Long cycle voltammetry curves of zinc-manganese batteries assembled with (25% NC) and comparative examples as positive electrode materials;

[0035] Fig.13 The MnO prepared in Example 1 2 (25% N), MnO 2 The first cyclic voltammetry curve of zinc-manganese battery assembled with (25% NC) and comparative example as positive electrode materials;

[0036] Fig.14 The MnO prepared in Example 1 2 (25% N), MnO 2 Ion diffusion proof diagram of the discharge process of zinc-manganese battery assembled with (25% NC) and comparative example as positive electrode materials;

[0037] Fig.15 The MnO prepared in Example 1 2 (25% N), MnO 2 (25% NC) and the comparative example are rate performance diagrams of zinc-manganese batteries assembled with positive electrode materials. DETAILED DESCRIPTION

[0038] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0039] Example 1

[0040] A method for preparing a positive electrode material for a battery comprises the following steps:

[0041] S1: Select three steel balls with diameters of 15 mm, 5 mm, and 3 mm, weigh their total mass to be 14.6 g, weigh 1.37 g of manganese dioxide, and 0.455 g of carbon amide, mix them evenly, put the steel balls and the mixture into a ball mill, add 6.9 g of deionized water, set the speed to 360 r / min, and ball mill for 28 h. After the ball milling is completed, filter the mixture, wash it, and place it in a drying oven at 150 ° C for 10 h to obtain MnO 2 (25%N);

[0042] S2: Select three steel balls with diameters of 15, 5, and 3 mm respectively, weigh their total mass to be 14.6 g, and weigh MnO 2 (25% N) 1.64g, conductive carbon black 0.185g were mixed evenly, steel balls and the mixture were put into a ball mill, and 8.2g of deionized water was added. The speed was set to 400r / min, and the ball milling was performed for 36h. After the ball milling was completed, the mixture was filtered, washed, and placed in a drying oven at 70℃ for 20h to obtain the battery positive electrode material MnO 2 (25% NC).

[0043] Example 2

[0044] A method for preparing a positive electrode material for a battery comprises the following steps:

[0045] S1: Select three steel balls with diameters of 15 mm, 5 mm, and 3 mm, weigh their total mass to be 14.6 g, weigh 1.64 g of manganese dioxide, and 0.185 g of carbon amide, mix them evenly, put the steel balls and the mixture into a ball mill, add 8.2 g of deionized water, set the speed to 300 r / min, and ball mill for 48 h. After the ball milling is completed, filter the mixture, wash it, and place it in a drying oven at 100 ° C for 12 h to obtain MnO 2 (10%N);

[0046] S2: Select three steel balls with diameters of 15, 5, and 3 mm respectively, weigh their total mass to be 14.6 g, and weigh MnO 2 (10% N) 1.62g, conductive carbon black 0.205g mixed evenly, put the steel ball and the mixture into the ball mill, add 8.1g deionized water, set the speed to 300r / min, ball mill for 48h, after the ball milling is completed, the mixture is filtered, washed, placed in a drying oven at 50℃ and dried for 24h to obtain the battery positive electrode material MnO2 (10% NC).

[0047] Example 3

[0048] A method for preparing a positive electrode material for a battery comprises the following steps:

[0049] S1: Select three steel balls with diameters of 15 mm, 5 mm, and 3 mm, weigh their total mass to be 14.6 g, weigh 1.46 g of manganese dioxide, and 0.365 g of carbonamide, mix them evenly, put the steel balls and the mixture into a ball mill, add 7.3 g of deionized water, set the speed to 500 r / min, and ball mill for 24 h. After the ball milling is completed, filter the mixture, wash it, and place it in a drying oven at 200 ° C for 8 h to obtain MnO 2 (20%N);

[0050] S2: Select three steel balls with diameters of 15, 5, and 3 mm respectively, weigh their total mass to be 14.6 g, and weigh MnO 2 (20% N) 1.64g, conductive carbon black 0.185g mixed evenly, put the steel ball and the mixture into the ball mill, add 8.2g deionized water, set the speed to 500r / min, ball mill for 24h, after the ball milling is completed, the mixture is filtered, washed, placed in a drying oven at 100℃ for 16h, and the battery positive electrode material MnO is obtained. 2 (20% NC).

[0051] Example 4

[0052] A method for preparing a positive electrode material for a battery comprises the following steps:

[0053] S1: Select three steel balls with diameters of 15 mm, 5 mm, and 3 mm, weigh their total mass to be 14.6 g, weigh 1.28 g of manganese dioxide, and 0.545 g of carbonamide, mix them evenly, put the steel balls and the mixture into a ball mill, add 6.4 g of deionized water, set the speed to 360 r / min, and ball mill for 28 h. After the ball milling is completed, filter the mixture, wash it, and place it in a drying oven at 150 ° C for 10 h to obtain MnO 2 (30%N);

[0054] S2: Select three steel balls with diameters of 15, 5, and 3 mm respectively, weigh their total mass to be 14.6 g, and weigh MnO 2 (30% N) 1.68g, conductive carbon black 0.145g were mixed evenly, steel balls and the mixture were put into a ball mill, and 8.4g of deionized water was added. The speed was set to 400r / min, and the ball milling was performed for 36h. After the ball milling was completed, the mixture was filtered, washed, and placed in a drying oven at 70℃ for 20h to obtain the battery positive electrode material MnO 2 (30% NC).

[0055] Comparative Example

[0056] Untreated MnO 2 powder.

[0057] Experimental Example 1

[0058] XRD characterization analysis of materials with different doping nitrogen source ratios: MnO prepared in Examples 1 to 4 2 (25% N), MnO 2 (10%N), MnO 2 (20%N), MnO 2 (30% N) and MnO of the comparative example 2 The experimental results are shown in Figure 2. Figure 1 As shown, all the diffraction peaks of the materials with different doping nitrogen source ratios are generally consistent with the manganese dioxide main material. Only when doping occurs, the peaks of the manganese dioxide main material are shifted and the peaks shrink or expand. No impurity peaks are seen, indicating that the prepared materials with different doping nitrogen source ratios have been successfully doped.

[0059] Experimental Example 2

[0060] XRD characterization analysis of materials with a nitrogen source ratio of 25%: MnO prepared in Example 1 2 (25% N), MnO 2 (25% NC) and MnO of the comparative example 2 The experimental results are shown in Figure 2. Figure 2 As shown, MnO 2 (25%N) and MnO 2 (25% NC) All diffraction peaks are roughly consistent with the main material of manganese dioxide. Only when doped, the peak of the main material of manganese dioxide is shifted and the peak shrinks or expands. No impurity peak is observed. The peak of conductive carbon black is located at MnO 2 (25% NC) is the second peak from left to right, and MnO 2 (25% N) is the second peak from left to right, indicating that the prepared MnO 2 (25% NC) materials have been successfully prepared;

[0061] Experimental Example 3

[0062] Crystal structure analysis of materials with a nitrogen source ratio of 25%: MnO prepared in Example 1 2 (25% NC) and MnO of the comparative example 2 Using transmission electron microscopy analysis, the experimental results are as follows Figures 3 to 6 As shown, by 2 Comparison of crystal phase structures before and after modification. Under a specific ball milling process, MnO obtained after nitrogen source doping2 The (25% NC) crystal phase structure has changed, which is beneficial to changing the cycle stability and discharge capacity of the manganese dioxide raw material when assembling the battery.

[0063] Experimental Example 4

[0064] Elemental morphology analysis of materials with a nitrogen source ratio of 25%: MnO prepared in Example 1 2 The surface of (25% NC) was scanned by scanning electron microscopy and elemental analysis was performed using an energy spectrum diffractometer. The experimental results are shown in Figures 7-8 As shown, EDS mapping shows the element distribution, and SEM images of MnO 2 The local size of 2μm and 500nm (25% NC) shows that nitrogen is present in MnO 2 (25% NC) was evenly distributed, indicating that nitrogen doping was successful.

[0065] Experimental Example 5

[0066] Conductivity analysis: All spin-polarized density functional theory (DFT) calculations were performed using VASP, and the generalized gradient approximation (GGA) and Perdew-Burke-Ernzerhof (PBE) formalisms were used to analyze the MnO prepared in Example 1. 2 (25% NC) and MnO of the comparative example 2 Modeling is performed and the obtained state density diagram is as follows Figures 9-10 As shown in the figure, it can be seen that the state density peak at the Fermi level is significantly enhanced after N element doping, so the conductivity is enhanced, that is, MnO 2 The conductivity of (25% NC) is stronger than that of MnO 2 .

[0067] Experimental Example 6

[0068] Battery performance experiment 1:

[0069] S1: MnO prepared in Examples 1 to 4 2 (25% N), MnO 2 (10%N), MnO 2 (20%N), MnO 2 (30% N) and graphene and polyvinylidene fluoride binder are mixed in a mass ratio of 7:2:1, and then N-methylpyrrolidone solvent is added and ground for 5 minutes to obtain a mixed slurry (the material-liquid ratio of the mixed material to the N-methylpyrrolidone solvent is 5g:1mL), and the mixed slurry is coated on carbon paper and dried at 60°C and then cooled to room temperature to obtain a battery positive electrode;

[0070] S2: The battery positive electrode is made of zinc sheet as negative electrode and glass fiber as separator, which is placed in the CR2032 battery shell and the electrolyte (ZnSO 4 With MnSO 4 , ZnSO 4 With MnSO 4 The molar ratio is 10:1), and the assembly of the aqueous zinc-manganese battery is completed after sealing.

[0071] The assembled battery was cycle tested on a battery testing system with a current of 1A g -1 , taking the first 1000 cycles of all battery cycles as comparison, the experimental results are as follows Fig.11 As shown, MnO 2 The battery with (25% N) as the positive electrode material has the best performance.

[0072] Experimental Example 7

[0073] Battery performance experiment 2:

[0074] S1: MnO prepared in Example 1 2 (25% N), MnO 2 (25% NC) and the comparative example are mixed with graphene and polyvinylidene fluoride binder in a mass ratio of 7:2:1, and then N-methylpyrrolidone solvent is added and ground for 5 minutes to obtain a mixed slurry (the material-liquid ratio of the mixed material to the N-methylpyrrolidone solvent is 5g:1mL), and the mixed slurry is coated on carbon paper and dried at 60°C and then cooled to room temperature to obtain a battery positive electrode;

[0075] S2: The battery positive electrode is made of zinc sheet as negative electrode and glass fiber as separator, which is placed in the CR2032 battery shell and the electrolyte (ZnSO 4 With MnSO 4 , ZnSO 4 With MnSO 4 The molar ratio is 10:1), and the assembly of the aqueous zinc-manganese battery is completed after sealing.

[0076] The assembled battery was cycle tested on a battery testing system with a current of 1A g -1 , taking the first 1000 cycles of all battery cycles as comparison, the experimental results are as follows Fig.12 As shown, MnO 2 The battery with (25% NC) as the positive electrode material has the best performance, indicating that the addition of conductive carbon black can further improve the performance of the battery, and also indicates that the addition of conductive carbon black can further improve the performance of the battery. 2 The modification was successful.

[0077] The first cyclic voltammetry curve of the assembled battery on the battery testing system is as follows: Fig.13 As shown, MnO2 The first turning point of the battery with (25% N) as the positive electrode material is compared with that of the battery with MnO 2 The first turning point of the battery with positive electrode material has a discharge capacity improvement of about 25% (the first turning point is H + The dominant electrochemical behavior) is MnO 2 The first turning point of the battery with (25% NC) as the positive electrode material is compared with that with MnO 2 The battery with MnO (25% N) as the positive electrode material has a 15% improvement in discharge capacity. 2 The second turning point of the battery with (25% N) as the positive electrode material is compared with that with MnO 2 The second turning point of the battery with positive electrode material has a discharge capacity improvement of about 33% (the second turning point is Zn 2+ The electrochemical behavior dominated by MnO 2 The second turning point of the battery with (25% NC) as the positive electrode material is compared with that with MnO 2 The battery with (25% N) as the positive electrode material has almost no significant improvement in discharge capacity, indicating that nitrogen doping can improve the H + ion diffusion behavior, but by MnO 2 (25% N) Adding conductive carbon black can not increase the Zn 2+ The ion diffusion behavior of Fig.14 shown.

[0078] By collecting the rate performance data of the battery in the cycle test, the rate performance diagrams of three types of batteries are obtained, such as Fig.15 As shown in the figure, the magnifications are 0.2C, 0.5C, 1C, 2C, 0.5C, and 0.2C respectively. It can be seen from the magnification diagram that MnO 2 The discharge performance of the battery with (25% NC) as the positive electrode material is the best, which also shows that MnO 2 The battery rate capability and cycle stability of (25% NC) are the best, indicating that the MnO 2 (25% NC) as the positive electrode material, the battery achieves ideal stable cycling and discharge capabilities.

[0079] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a positive electrode material for a battery, characterized in that: The following steps are involved: S1: manganese dioxide and a nitrogen source are prepared into a mixture in a mass ratio of 7-9:1-3, the mixture is ball-milled at a speed of 300-500 r / min for 24-48 hours, and the ball-milled mixture is washed and dried at 100-200° C. for 8-12 hours to obtain a crude product; S2: The crude product and the carbon source are combined into a mixture 2 in a mass ratio of 8 to 12:1, and the mixture 2 is ball-milled at a speed of 300 to 500 r / min for 24 to 48 hours. The ball-milled mixture 2 is then washed and dried at 50 to 100° C. for 16 to 24 hours to obtain the mixture.

2. The method for preparing a positive electrode material for a battery according to claim 1, wherein: The nitrogen source is carbonamide, and the carbon source is conductive carbon black.

3. The method for preparing a positive electrode material for a battery according to claim 1, wherein: In S1, the ball mill uses water with a mass 5 times that of manganese dioxide as the medium, a ball-to-material ratio of 8:1, a rotation speed of 360 r / min, a ball milling time of 28 h, a drying temperature of 150°C, and a drying time of 10 h.

4. The method for preparing a positive electrode material for a battery according to claim 1, wherein: In S2, the ball mill uses water 5 times the mass of the crude product as the medium, the ball-to-material ratio is 8:1, the rotation speed is 400 r / min, the ball milling time is 36 h, the drying temperature is 70°C, and the drying time is 20 h.

5. The battery positive electrode material prepared by the method for preparing the battery positive electrode material according to any one of claims 1 to 5.

6. Use of the battery positive electrode material according to claim 6 in the preparation of zinc-manganese batteries.

7. The use according to claim 6, characterized in that The zinc-manganese battery is prepared by the following steps: S1: The battery positive electrode material, graphene and binder are prepared into a mixture in a mass ratio of 7:2:1, and then a solvent is added and ground for 5 minutes to obtain a mixed slurry. The mixed slurry is coated on carbon paper and dried at 60°C and then cooled to room temperature to obtain a battery positive electrode; the material-liquid ratio of the mixture three to the solvent is 5g:1mL. S2: Using zinc sheet as negative electrode and glass fiber as separator, the prepared battery positive electrode is placed in the battery shell, electrolyte is added, and the zinc-manganese battery is assembled after sealing; the electrolyte composition is ZnSO4 and MnSO4, and the molar ratio of ZnSO4 to MnSO4 is 10:

1.

8. The use according to claim 7, characterized in that: The binder described in S1 is polyvinylidene fluoride, and the solvent is N-methylpyrrolidone.