Positive electrode composite material, positive electrode containing positive electrode composite material and preparation method of positive electrode

By adding inorganic lithium salts to p-type organic materials, the electrochemical performance of the lithium-ion battery cathode is improved, solving the problem of low electrochemical performance of p-type organic materials in the existing technology, and achieving more efficient energy storage and simplified preparation process.

CN118738388AActive Publication Date: 2024-10-01BEIHANG UNIV

Patent Information

Application Number
CN202410753989.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

In the existing technology, p-type organic materials have low electrochemical performance when used as the cathode of lithium-ion batteries, especially at high potentials, and the utilization rate of active sites is low, which needs improvement.

Method used

Inorganic lithium salts, such as lithium phosphate, are added to p-type organic materials, combined with conductive agents and binders to prepare a positive electrode composite material. Lithium-ion battery positive electrodes are prepared through specific grinding and drying steps to improve p-type doping. concentration and active site utilization.

Benefits of technology

It significantly improves the electrochemical performance of p-type organic energy storage materials, improves the energy storage performance of lithium-ion batteries, simplifies the preparation process, and provides a broader development space.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738388A_ABST
    Figure CN118738388A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode composite material, a positive electrode containing the positive electrode composite material and a preparation method of the positive electrode, and relates to the technical field of electrochemical materials. The invention provides a positive electrode composite material. The positive electrode composite material comprises a p-type organic material, an inorganic lithium salt, a conductive agent and a binder, the inorganic lithium salt is selected from one or a mixture of more of lithium phosphate, lithium carbonate, lithium fluoride and lithium sulfate. The inorganic lithium salt is creatively added into the p-type organic material, so that the p-type doping concentration of the organic material is effectively improved, the active site utilization rate and the specific capacity of the p-type organic material are further improved, and the electrochemical performance of the p-type organic energy storage material is remarkably improved; the lithium ion battery positive plate prepared from the positive electrode composite material provided by the invention has the advantages of mild preparation conditions and simple process while greatly improving the energy storage performance of the battery, and has wider development space compared with the traditional lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical materials, and in particular to a positive electrode composite material, a positive electrode containing the positive electrode composite material, and a preparation method thereof. Background Art

[0002] At present, traditional lithium-ion batteries are reversibly charged and discharged by lithium ions shuttling back and forth between the positive electrode and the negative electrode. When organic materials are used as the positive electrode of lithium-ion batteries, they can be divided into n-type organic materials, p-type organic materials and bipolar organic materials according to the energy storage principle. The energy storage principle of n-type organic materials is the reversible embedding and extraction of lithium ions in the positive electrode, and the energy storage principle of p-type organic materials (POM) is the reversible embedding and extraction of anions in the electrolyte in the positive electrode. Bipolar materials have both n-type and p-type energy storage characteristics, combining cations at low voltages and anions at high voltages.

[0003] The molecular formula of lithium phosphate is Li3P04, which is a white crystalline powder of orthorhombic system, and is easily soluble in dilute acid and slightly soluble in water. It is an important electrolyte additive; due to its special catalytic and electrochemical properties, it is widely used in the field of electrochemical materials.

[0004] N,N,N,N-tetraphenyl-1,4-phenylenediamine (TPPA) is an organic small molecule with two graphitic nitrogen atoms. After electrochemical p-type doping, the degree of free radical delocalization is high and the intermediate is relatively stable. It is an ideal p-type organic small molecule with a theoretical specific capacity of 130 mAh g -1 However, in practical applications, when it is used as a positive electrode material for lithium-ion batteries, its performance is much different from the theoretical specific capacity. This is because when it is charged by p-type doping, the anions in the electrolyte are large in volume, and the steric hindrance when inserted into / out of the electrode during the charge and discharge process is large, which inhibits the reaction kinetics and reduces the utilization rate and specific capacity of the active sites of the organic electrode material.

[0005] Covalent triazine framework (CTF) is a p-type organic porous polymer containing triazine rings. It has abundant active sites, large specific surface area, good durability and good conductivity, and has been widely used in various energy storage devices. When used as an electrode material, triazine ring has bipolar characteristics. It can not only perform n-type doping energy storage at low potential, but also be converted into triazine radical cations combined with anions at high potential for p-type doping energy storage. However, when CTFs are used as positive electrodes, the utilization rate of active sites is low when p-type doping is performed through anion compensation of the electrolyte at high potential, and further improvement is needed. In view of this, it is very necessary to develop a positive electrode composite material based on p-type organic materials to improve the electrochemical performance of lithium-ion batteries. Summary of the invention

[0006] The object of the present invention is to provide a positive electrode composite material and a positive electrode containing the positive electrode composite material and a preparation method thereof, so as to solve the technical problem in the prior art that the electrochemical performance of p-type organic materials as battery positive electrodes is not high.

[0007] In order to solve the above technical problems, the present invention provides a positive electrode composite material, including a p-type organic material, an inorganic lithium salt, a conductive agent, and a binder;

[0008] The inorganic lithium salt is selected from one or more mixtures of lithium phosphate, lithium carbonate, lithium fluoride and lithium sulfate; preferably lithium phosphate.

[0009] The addition of non-polar lithium salts can improve the energy storage performance of p-type organic materials and further improve the electrochemical performance of lithium-ion batteries.

[0010] Further, the p-type organic material is selected from p-type organic small molecules and / or p-type organic polymers;

[0011] Preferably, the p-type organic small molecule material is N,N,N,N-tetraphenyl-1,4-phenylenediamine;

[0012] Preferably, the p-type organic polymer is a covalent triazine-based framework.

[0013] Furthermore, the amount of the inorganic lithium salt added should not be higher than 4 times the total mass of the p-type organic material;

[0014] Furthermore, the conductive agent is selected from one or more mixtures of carbon nanotubes, acetylene black, graphene, Ketjen black, and carbon black, preferably Ketjen black.

[0015] Furthermore, the binder is selected from one or more mixtures of polyvinylidene fluoride, carboxymethyl cellulose, polytetrafluoroethylene, styrene-butadiene rubber, preferably polyvinylidene fluoride.

[0016] The present invention provides a lithium ion battery positive electrode, comprising a current collector and the positive electrode composite material;

[0017] The current collector is selected from any one of metal foil, foam metal material and carbon-coated metal material.

[0018] On the other hand, the present invention provides a method for preparing a positive electrode of a lithium ion battery, the specific steps are as follows:

[0019] Step 1, weighing a p-type organic material, a conductive agent, a binder, and an inorganic lithium salt in a certain mass ratio, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar to obtain a grinding slurry with uniform particles;

[0020] Step 2: Take the grinding slurry, evenly coat it on the surface of the current collector, dry it in a vacuum oven at 80-90° C., and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0021] Furthermore, in step 1, the mass ratio of the p-type organic material, the conductive agent, the binder, and the inorganic lithium salt is (3-7): (2-6): 1: (1-28).

[0022] Furthermore, the grinding time in step 1 is 30-60 min.

[0023] Furthermore, the drying time in step 2 is 20-24 hours, preferably 24 hours.

[0024] By adopting the above technical solution, the present invention has the following beneficial effects:

[0025] The present invention provides a positive electrode composite material, which creatively adds an inorganic lithium salt to a p-type organic material, effectively increasing the p-type doping concentration of the organic material, thereby improving the active site utilization and specific capacity of the p-type organic material, and significantly improving the electrochemical performance of the p-type organic energy storage material; the lithium ion battery positive electrode prepared using the positive electrode composite material provided by the present invention, while greatly improving the battery energy storage performance, also has the advantages of mild preparation conditions and simple process, and has a broader development space compared with traditional lithium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A schematic diagram of the working principle of the lithium-ion battery positive electrode composite material provided by the present invention;

[0028] Figure 2 This is the cycle performance curve of TPPA material as the positive electrode of lithium-ion battery;

[0029] Figure 3 This is the cycle performance curve of TPPA@Li3PO4 material as the positive electrode of lithium-ion battery;

[0030] Figure 4 The cycle performance curves of CTF material and CTF@Li3PO4 material as positive electrode of lithium-ion battery;

[0031] Figure 5This is a comparison chart of the rate performance of CTF material and CTF@Li3PO4 material as positive electrode of lithium-ion battery;

[0032] Figure 6 The discharge curve of TPPA as the positive electrode of lithium-ion battery, as well as the capacity ratio of n-type doping and p-type doping;

[0033] Figure 7 The discharge curve of TPPA@Li3PO4 as the positive electrode of lithium-ion battery, as well as the capacity ratio of n-type doping and p-type doping;

[0034] Figure 8 The discharge curve when CTF is used as the positive electrode of lithium-ion battery, as well as the capacity ratio diagram of n-type doping and p-type doping;

[0035] Fig. 9 This is the discharge curve when CTF@Li3PO4 is used as the positive electrode of a lithium-ion battery, as well as the capacity ratio of n-type doping and p-type doping. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The present invention is further explained below in conjunction with specific implementation modes.

[0038] The specific steps of preparing a positive electrode sheet of a lithium-ion battery using the lithium-ion battery positive electrode composite material provided by the present invention are as follows:

[0039] Step S1, weighing a p-type organic material, a conductive agent, a binder, and an inorganic lithium salt in a mass ratio of (3-7): (2-6): 1: (1-28), adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 30-60 minutes to obtain a grinding slurry with uniform particles;

[0040] Step 2: Take the grinding slurry, evenly coat it on the surface of the current collector, vacuum dry it at 80-90° C. for 20-24 hours, and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0041] like Figure 1 As shown, during the charge and discharge process, the positive electrode containing the positive electrode composite material provided by the present invention is charged by anions with relatively high charge mass (such as PO4 3- 、CO3 2- 、F - ) to replace PF6 in the original electrolyte- Anions avoid the defect of traditional p-type organic cathodes that need to embed or remove larger anions in order to store energy during the charge and discharge process, thereby balancing the positive charge carried by the cations in the oxidized state of the p-type organic cathode, making Li+ ions the main carrier. This will significantly reduce the steric hindrance of ion migration and occupation, and increase the Li + quantity, improving reaction kinetics and specific capacity.

[0042] Example 1

[0043] This example verifies a method for preparing a TPPA@Li3PO4 composite material and simultaneously preparing a positive electrode sheet for a lithium-ion battery using an organic small molecule N,N,N,N-tetraphenyl-1,4-phenylenediamine (TPPA) as a raw material.

[0044] Step S1, weighing TPPA material, Ketjen black, polyvinylidene fluoride (PVDF), and lithium phosphate in a mass ratio of 5:4:1:1, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 30 minutes to obtain a grinding slurry with uniform particles;

[0045] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 80-90° C. for 24 hours, and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0046] Comparative Example 1

[0047] In this comparative example, N,N,N,N-tetraphenyl-1,4-phenylenediamine organic small molecule (TPPA) is used as a raw material to prepare a positive electrode sheet for a lithium ion battery without adding an inorganic lithium salt.

[0048] Step S1, weighing TPPA material, Ketjen black, and polyvinylidene fluoride (PVDF) in a mass ratio of 5:4:1, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 30 minutes to obtain a grinding slurry with uniform particles;

[0049] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 80° C. for 24 hours, and cut it to obtain a TPPA lithium-ion battery positive electrode sheet that does not contain inorganic lithium salt.

[0050] Example 2

[0051] This example verifies the method of using triazine framework (CTF) as raw material to prepare CTF@Li3PO4 composite material and simultaneously prepare lithium-ion battery positive electrode sheet.

[0052] Step S1, weighing CTF material, Ketjen black, polyvinylidene fluoride (PVDF), and lithium phosphate in sequence according to a mass ratio of 6:3:1:1, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 60 minutes to obtain a grinding slurry with uniform particles;

[0053] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 80-90° C. for 24 hours, and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0054] Comparative Example 2

[0055] In this comparative example, a triazine framework (CTF) is used as a raw material to prepare a positive electrode sheet for a lithium-ion battery without adding an inorganic lithium salt.

[0056] Step S1, weighing CTF material, Ketjen black, and polyvinylidene fluoride (PVDF) in a mass ratio of 6:3:1, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 60 minutes to obtain a grinding slurry with uniform particles;

[0057] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 90° C. for 20 hours, and cut it to obtain a CTF lithium-ion battery positive electrode sheet that does not contain inorganic lithium salt.

[0058] Example 3

[0059] This example verifies the addition of different types of inorganic lithium salts to prepare positive electrodes for lithium-ion batteries.

[0060] Step S1, weighing CTF material, carbon black, polyvinylidene fluoride (PVDF), and lithium carbonate in a mass ratio of 5:4:1:12, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 60 minutes to obtain a grinding slurry with uniform particles;

[0061] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 80-90° C. for 24 hours, and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0062] Example 4

[0063] This example verifies the use of different amounts of inorganic lithium salts to prepare positive electrodes for lithium-ion batteries.

[0064] Step S1, weighing TPPA material, carbon black, polyvinylidene fluoride (PVDF), and lithium hexafluorophosphate in a mass ratio of 6:3:1:20, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar for 50 minutes to obtain a grinding slurry with uniform particles;

[0065] Step 2: Take the grinding slurry, evenly coat it on the carbon-coated aluminum foil, vacuum dry it at 80-90° C. for 20 hours, and cut it to obtain a lithium-ion battery positive electrode sheet containing the positive electrode composite material.

[0066] Example 5

[0067] like Figure 2-Figure 3 As shown, through comparative experiments, the cycle performance of lithium-ion batteries assembled with two battery positive electrode sheets prepared in Example 1 and Comparative Example 1 was tested:

[0068] The battery positive electrode sheet and the metal lithium sheet prepared in Example 1 and Comparative Example 1 were respectively used as the battery negative electrode, and 1MLiPF6 EC / DEC (v:v=1:1) was used as the electrolyte to assemble two groups of CR2032 button half-cells, which were marked as TPPA@Li3PO4 battery and TPPA battery respectively.

[0069] The battery cycle performance was tested by constant current charge and discharge at a current density of 1A / g. The results are as follows:

[0070] like Figure 2 As shown in FIG. 1 , after 300 cycles at 1 A / g, the capacity of the TPPA battery prepared in Comparative Example 1 is only 69.1 mAh / g, while under the same test conditions, a certain amount of lithium phosphate is added during the preparation process of the TPPA@Li3PO4 battery, such as Figure 3 As shown in the figure, its capacity can reach 124mAh / g. It can be seen that when using p-type organic small molecules as the positive electrode raw materials of lithium batteries, adding inorganic lithium salts can effectively improve the cycle performance of the battery.

[0071] Example 6

[0072] like Figure 4 As shown, through comparative experiments, the cycle performance of lithium-ion batteries assembled with two battery positive electrode sheets prepared in Example 2 and Comparative Example 2 was tested:

[0073] The battery positive electrode sheet and the metal lithium sheet prepared in Example 2 and Comparative Example 2 were respectively used as the battery negative electrode, and 1MLiPF6 EC / DEC (v:v=1:1) was used as the electrolyte to assemble two groups of CR2032 button half-cells, which were marked as CTF@Li3PO4 battery and CTF battery respectively.

[0074] The battery cycle performance was tested by constant current charge and discharge at a current density of 0.1A / g. The results are as follows:

[0075] like Figure 4As shown in the figure, after 300 cycles at 0.1A / g, the capacity of the CTF battery prepared in Comparative Example 2 is 75.4mAh / g; while under the same test conditions, the capacity of the CTF@Li3PO4 battery with a certain amount of lithium phosphate added during the preparation process can reach 89mAh / g. It can be seen that when using p-type organic polymer as the positive electrode raw material of lithium battery, the addition of inorganic lithium salt can also effectively improve the cycle performance of the battery.

[0076] It can be seen from the test results of Examples 5-6 above that for lithium-ion battery positive electrodes made of p-type organic materials, adding an appropriate amount of inorganic lithium salt during the preparation process can significantly improve the cycle performance of lithium-ion batteries assembled using the positive electrodes.

[0077] Example 7

[0078] like Figure 5 As shown, the rate performance of different lithium-ion battery positive electrodes prepared in Example 2 and Comparative Example 2 was tested:

[0079] The battery positive electrode sheet and the metal lithium sheet prepared in Example 2 and Comparative Example 2 were respectively used as the battery negative electrode, and 1MLiPF6 EC / DEC (v:v=1:1) was used as the electrolyte to assemble two groups of CR2032 button half-cells, which were marked as CTF@Li3PO4 battery and CTF battery respectively.

[0080] The battery was charged and discharged at constant current density of 0.1, 0.2, 0.5, 1, 2, 5, and 10 A / g, and the discharge capacity was tested. The results are as follows: Figure 5 As shown in Table 1,

[0081] Table 1 Comparison of discharge capacity of CTF battery and CTF@Li3PO4 battery:

[0082]

[0083] It can be seen from Table 1 that as the current density increases, the discharge capacity of the battery decreases accordingly, but the discharge capacity of the CTF@Li3PO4 battery is always higher than that of the CTF battery. It can be seen that the present invention provides a positive electrode composite material, because a proper amount of inorganic lithium salt is added to the p-type organic material, which can significantly improve the electrochemical performance of a lithium ion battery using it as a positive electrode.

[0084] Example 8

[0085] like Figure 6-Figure 9 As shown, this embodiment verifies the improvement of battery performance by adding inorganic lithium salts by studying the discharge curves of four batteries assembled with the positive electrode sheets prepared by Examples 1-2 and Comparative Examples 1-2 and determining the capacity ratio of n-type doping and p-type doping.

[0086] The positive electrode sheet and metal lithium sheet prepared in Example 1, Comparative Example 1, Example 2 and Comparative Example 2 were used as the negative electrode of the battery, and 1M LiPF6 EC / DEC (v:v=1:1) was used as the electrolyte to assemble four groups of CR2032 button half-cells, which were marked as TPPA@Li3PO4 battery, TPPA battery, CTF@Li3PO4 battery, and CTF battery. At a current density of 1A / g, the discharge curve of the 300th cycle was recorded; the discharge curve was horizontally divided at the voltage node 3.0V of the n / p type energy storage, and the specific capacity corresponding to the horizontal axis was obtained. Figure 6-Figure 9 .from Figure 6-Figure 9 In the table 2, we can get the data:

[0087] Table 2 Comparison of p-type capacity of the above four batteries

[0088] Battery Type p-type capacity ratio (mAh / g) TPPA battery 39.7 <![CDATA[TPPA@Li3PO4 battery]]> 77.1 CTF Battery 46.5 <![CDATA[CTF@Li3PO4 battery]]> 55.9

[0089] It can be clearly seen from Table 2 that for the battery positive electrode sheet using the same p-type organic material as the raw material, the p-type capacity ratio of the battery with the inorganic lithium salt added is significantly higher than that without the addition. It can be seen that the positive electrode composite material provided by the present invention improves the utilization rate of the p-type active sites of the p-type organic material by adding the inorganic lithium salt, thereby improving the energy storage performance of the p-type organic material, and achieving the technical effect of significantly improving the electrochemical performance of the p-type organic material when used as the positive electrode of the battery.

[0090] In summary, the positive electrode composite material provided by the present invention can effectively improve the utilization rate of p-type active sites and enhance the performance of p-type organic energy storage materials by adding an appropriate amount of inorganic lithium salt to p-type organic materials. The positive electrode sheet prepared using the above composite material has a relatively broad application space in the field of lithium-ion batteries.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode composite material, characterized in that: The composite material comprises a p-type organic material, an inorganic lithium salt, a conductive agent, and a binder; The inorganic lithium salt is selected from one or more mixtures of lithium phosphate, lithium carbonate, lithium fluoride and lithium sulfate.

2. The positive electrode composite material according to claim 1, characterized in that: The p-type organic material is selected from p-type organic small molecules and / or p-type organic polymers.

3. The positive electrode composite material according to claim 1, characterized in that: The added amount of the inorganic lithium salt is no more than 4 times the total mass of the p-type organic material.

4. The positive electrode composite material according to claim 1, characterized in that: The conductive agent is selected from one or more mixtures of carbon nanotubes, acetylene black, graphene, Ketjen black, and carbon black.

5. The positive electrode composite material according to claim 1, characterized in that: The adhesive is selected from one or more mixtures of polyvinylidene fluoride, carboxymethyl cellulose, polytetrafluoroethylene, and styrene-butadiene rubber.

6. A positive electrode for a lithium ion battery, characterized in that: The positive electrode sheet comprises a current collector and the positive electrode composite material according to any one of claims 1 to 5; The current collector is selected from any one of metal foil, foam metal material and carbon-coated metal material.

7. A method for preparing a positive electrode for a lithium ion battery according to claim 6, characterized in that: The specific steps are as follows: Step 1, weighing a p-type organic material, a conductive agent, a binder, and an inorganic lithium salt in a certain mass ratio, adding them to a solvent of N-methylpyrrolidone, and grinding them in a mortar to obtain a grinding slurry with uniform particles; Step 2: Take the grinding slurry, evenly coat it on the surface of the current collector, dry it in a vacuum oven at 80-90° C., and cut it to obtain a lithium-ion battery positive electrode containing the positive electrode composite material.

8. The preparation method according to claim 7, characterized in that: The mass ratio of the p-type organic material, the conductive agent, the binder and the inorganic lithium salt in step 1 is (3-7): (2-6): 1: (1-28).

9. The preparation method according to claim 7, characterized in that: The grinding time in step 1 is 30-60 min.

10. The preparation method according to claim 7, characterized in that: The drying time in step 2 is 20-24 hours.

Citation Information

Patent Citations

  • Lithium iron conductive complex modified lithium iron phosphate anode material and preparation method thereof

    CN103022484A

  • All-organic magnesium ion battery and preparation method thereof

    CN108470940A

  • Double-ion embedded type cross-linked triphenylamine polymer lithium ion battery positive pole material and preparation method thereof

    CN110350193A

  • Electrode plate, preparation method thereof and secondary battery formed by electrode plate

    CN114566611A

  • Nitrogen-containing organic positive electrode material and preparation method and application thereof

    CN115745972A

Cited By

  • Rechargeable potassium ion battery

    US12802987B2