Membrane electrode and preparation method and application thereof
By using modified Nafion membrane and surface-modified g-C3N4-SO3H in hydrogen-oxygen fuel cell membrane electrodes, combined with platinum salt and sodium borohydride treatment, the problem of gas/liquid mass transfer obstruction in traditional membrane electrodes is solved and the proton efficiency is improved. transmission performance and electrocatalyst utilization, achieving more efficient energy conversion.
Patent Information
- Application Number
- CN202411108568.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-01
AI Technical Summary
The dense catalytic layer structure of traditional hydrogen-oxygen fuel cell membrane electrodes hinders gas/liquid mass transfer, resulting in reduced electrocatalyst utilization, and ionomers occupy catalytically active sites, affecting proton transport performance.
Using a modified Nafion membrane, the surface is doped with surface-modified g-C3N4-SO3H, and there is no binder in the membrane electrode. It is combined with soluble platinum salt and sodium borohydride aqueous solution to form a high electronic conductivity. and membrane electrodes with excellent proton transport properties.
It improves the active sites and electronic conductivity of the membrane electrode, reduces the catalytic layer/membrane interface resistance, promotes proton transport, and improves the energy conversion efficiency of the fuel cell.
Smart Images

Figure HDA0004991518940000011 
Figure HDA0004991518940000012 
Figure HDA0004991518940000013
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a membrane electrode and a preparation method and application thereof. Background Art
[0002] Fuel cells use clean energy such as hydrogen and methanol as fuel, and directly convert chemical energy into electrical energy through redox reactions. They have the advantages of high energy conversion efficiency, harmless reaction products, and low environmental pollution. Hydrogen-oxygen fuel cells also have the advantages of low-temperature rapid start-up, high safety and reliability, and convenient maintenance. However, the dense catalytic layer structure of traditional hydrogen-oxygen fuel cell membrane electrodes obtained with catalytic inks hinders gas / liquid mass transfer, and ionomers occupy catalytic active sites, thereby reducing the utilization rate of electrocatalysts. Summary of the invention
[0003] The object of the present invention is to provide a membrane electrode and a preparation method and application thereof, wherein the membrane electrode has larger active sites and higher electronic conductivity and has excellent proton transport performance.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a membrane electrode, comprising a modified Nafion membrane and Pt located on the surface of the modified Nafion membrane;
[0006] The modified Nafion membrane is a g-C3N4-SO3H-doped Nafion membrane;
[0007] The g-C3N4-SO3H in the modified Nafion membrane is g-C3N4 with -SO3H surface modification;
[0008] The membrane electrode does not contain any binder.
[0009] Preferably, the mass percentage of g-C3N4-SO3H in the membrane electrode is 0 to 10%, and is not 0.
[0010] Preferably, the mass of Pt in the membrane electrode is 0.05-1.5 mg per square centimeter.
[0011] The present invention also provides a method for preparing the membrane electrode described in the above technical solution, comprising the following steps:
[0012] Sulfuric acid is added to the dispersion of g-C3N4 to modify it and obtain g-C3N4-SO3H;
[0013] Mixing the g-C3N4-SO3H and an organic solvent to obtain a dispersion of g-C3N4-SO3H;
[0014] Mixing the Nafion solution and the dispersion of g-C3N4-SO3H to obtain a film casting solution;
[0015] After the casting solution is formed into a film, it is boiled in a hydrogen peroxide solution, a sulfuric acid solution and water in sequence to obtain a g-C3N4-SO3H / Nafion membrane;
[0016] After the g-C3N4-SO3H / Nafion membrane is immersed in a soluble platinum salt solution, a sodium borohydride aqueous solution is added to obtain the membrane electrode.
[0017] Preferably, the concentration of the g-C3N4 dispersion is 0.1 to 10 g / L;
[0018] The concentration of the sulfuric acid is 0.01 to 5 mol / L;
[0019] The volume ratio of the g-C3N4 dispersion and sulfuric acid is (0.1-50):1.
[0020] Preferably, the modification is carried out under stirring conditions;
[0021] The stirring temperature is 293-363K, the rotation speed is 10-800 rpm, and the time is 3-24 hours.
[0022] Preferably, the organic solvent includes one or more of dimethyl sulfoxide, cyclohexane, N,N-dimethylformamide, toluene, ethanol and methanol;
[0023] The concentration of the g-C3N4-SO3H dispersion is 0.1 to 15 g / L.
[0024] Preferably, the mass concentration of g-C3N4-SO3H in the casting solution is 0 to 0.4%, and is not 0.
[0025] Preferably, the soluble platinum salt in the soluble platinum salt solution includes one or more of tetraammine dichloroplatinum, platinum dichloride, platinum tetrachloride, chloroplatinic acid and potassium chloroplatinate;
[0026] The concentration of the soluble platinum salt solution is 0 to 1 mmol / L, and is not 0;
[0027] The mass percentage concentration of the sodium borohydride aqueous solution is 0.1-10%;
[0028] The immersion temperature is 293-353K and the immersion time is 0.5-36h;
[0029] The process of adding the sodium borohydride aqueous solution is carried out under the condition of 298K.
[0030] The present invention also provides the use of the membrane electrode described in the above technical solution or the membrane electrode prepared by the preparation method described in the above technical solution in a fuel cell.
[0031] The present invention provides a membrane electrode, comprising a modified Nafion membrane and Pt located on the surface of the modified Nafion membrane; the modified Nafion membrane is a g-C3N4-SO3H-doped Nafion membrane; the g-C3N4-SO3H in the modified Nafion membrane is g-C3N4 with -SO3H surface modification; the membrane electrode does not contain an adhesive. The membrane electrode does not contain an adhesive, so that it has a larger active site and a higher electronic conductivity; at the same time, it has excellent gas / liquid mass transfer performance, thereby reducing the catalyst layer / membrane interface resistance and promoting proton transport at the interface. Among them, the role of the g-C3N4 surface modified with -SO3H is to serve as a proton conduction site to improve the proton conduction performance; the role of the Pt is to affect the proton conduction performance of the modified Nafion membrane with the catalyst layer as the membrane electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-1 described in Example 1 at 303K to 353K and 100% relative humidity;
[0033] Figure 2 The proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.3-0.5 described in Example 2 at 303K~353K and 100% relative humidity;
[0034] Figure 3 The proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-0.25 described in Example 3 at 303K~353K and 100% relative humidity;
[0035] Figure 4 The proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-1 described in Example 4 at 303K to 353K and 100% relative humidity;
[0036] Figure 5 The proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-0.25 described in Example 5 at 303K to 353K and 100% relative humidity;
[0037] Figure 6The proton conductivity curve of the integrated membrane electrode of Pt@Nafion-1 described in Comparative Example 1 at 303K to 353K and 100% relative humidity;
[0038] Figure 7 This is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4 / Nafion-0.4-1 described in Comparative Example 2 at 303K~353K and 100% relative humidity. DETAILED DESCRIPTION
[0039] The present invention provides a membrane electrode, comprising a modified Nafion membrane and Pt located on the surface of the modified Nafion membrane;
[0040] The modified Nafion membrane is a g-C3N4-SO3H-doped Nafion membrane;
[0041] The g-C3N4-SO3H in the modified Nafion membrane is g-C3N4 with -SO3H surface modification;
[0042] The membrane electrode does not contain any binder.
[0043] In the present invention, the mass percentage of g-C3N4-SO3H in the membrane electrode is preferably 0 to 10%, and is not 0, more preferably 0.01 to 5%, and most preferably 0.05 to 3%.
[0044] In the present invention, the mass of Pt in the membrane electrode per square centimeter is preferably 0.05 to 1.5 mg, more preferably 0.1 to 0.8 mg, and most preferably 0.2 to 0.6 mg. In the present invention, the particle size of Pt is preferably nanometer-scale.
[0045] In the present invention, the mass percentage of -SO3H in the g-C3N4-SO3H is preferably 0 to 20%, more preferably 0.5 to 15%, and most preferably 1 to 10%.
[0046] The present invention also provides a method for preparing the membrane electrode described in the above technical solution, comprising the following steps:
[0047] Sulfuric acid is added to the dispersion of g-C3N4 to modify it and obtain g-C3N4-SO3H;
[0048] Mixing the g-C3N4-SO3H and an organic solvent to obtain a dispersion of g-C3N4-SO3H;
[0049] Mixing the Nafion solution and the dispersion of g-C3N4-SO3H to obtain a film casting solution;
[0050] After the casting solution is formed into a film, it is boiled in a hydrogen peroxide solution, a sulfuric acid solution and water in sequence to obtain a g-C3N4-SO3H / Nafion membrane;
[0051] After the g-C3N4-SO3H / Nafion membrane is immersed in a soluble platinum salt solution, a sodium borohydride aqueous solution is added to obtain the membrane electrode.
[0052] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0053] The present invention adds sulfuric acid into the dispersion of g-C3N4 to modify it and obtain g-C3N4-SO3H.
[0054] In the present invention, the concentration of the dispersion of g-C3N4 is preferably 0.1-10 g / L, more preferably 0.3-8 g / L, and most preferably 0.5-4 g / L. In the present invention, the dispersion of g-C3N4 is preferably obtained by mixing g-C3N4 and water; the water is preferably deionized water; the present invention does not have any special restrictions on the source of the g-C3N4, and the source familiar to those skilled in the art can be used. In an embodiment of the present invention, the g-C3N4 is specifically prepared by a conventional preparation method using urea as a raw material. In the present invention, the mixing is preferably carried out under ultrasonic conditions, and the frequency of the ultrasound is preferably 300-8000 Hz, more preferably 500-6000 Hz, and most preferably 800-4000 Hz; the time of the ultrasound is preferably 5 min-6 h, more preferably 20 min-3 h, and most preferably 0.5-2 h.
[0055] In the present invention, the concentration of sulfuric acid is preferably 0.01 to 5 mol / L, more preferably 0.02 to 2 mol / L, and most preferably 0.1 mol / L.
[0056] In the present invention, the volume ratio of the g-C3N4 dispersion and sulfuric acid is preferably (0.1-50):1, more preferably (0.1-25):1, further preferably (0.5-15):1, and most preferably (1-10):1.
[0057] The present invention has no special limitation on the process of adding sulfuric acid, and the process well known to those skilled in the art can be used.
[0058] In the present invention, the modification is preferably carried out under stirring conditions, the stirring temperature is preferably 293-363K, more preferably 303-353K, most preferably 333K, the rotation speed is preferably 10-800rpm, more preferably 50-500rpm, most preferably 80-300rpm, the time is preferably 3-24h, more preferably 5-18h, most preferably 6-15h. In the present invention, the stirring is preferably magnetic stirring.
[0059] After the modification is completed, the present invention further preferably comprises evaporation. The present invention has no special limitation on the evaporation process, and the evaporation process can be performed using a process well known to those skilled in the art. In an embodiment of the present invention, the evaporation is specifically performed in a solution evaporator.
[0060] After obtaining the g-C3N4-SO3H, the present invention further comprises mixing the g-C3N4-SO3H with an organic solvent to obtain a dispersion of g-C3N4-SO3H.
[0061] In the present invention, the organic solvent preferably includes one or more of dimethyl sulfoxide, cyclohexane, N,N-dimethylformamide, toluene, ethanol and methanol. When the organic solvent is two or more of the above specific options, the present invention has no special limitation on the ratio of the above specific substances, and they can be mixed in any ratio.
[0062] In the present invention, the mixing is preferably carried out in the form of cell crushing. The present invention does not have any special restrictions on the conditions of the cell crushing, and the conditions well known to those skilled in the art can be used to uniformly disperse the g-C3N4-SO3H in the organic solvent within 90 minutes.
[0063] In the present invention, the concentration of the g-C3N4-SO3H dispersion is preferably 0.1 to 15 g / L, more preferably 0.5 to 10 g / L, further preferably 1 to 6 g / L, and most preferably 2.5 g / L.
[0064] After obtaining the dispersion of g-C3N4-SO3H, the present invention mixes the Nafion solution and the dispersion of g-C3N4-SO3H to obtain a casting solution.
[0065] In the present invention, the volume ratio of the Nafion solution to the dispersion of g-C3N4-SO3H is preferably (5-35):1, more preferably (10-28):1, and most preferably (18-25):1.
[0066] In the present invention, the mixing is preferably carried out under ultrasonic conditions. The present invention does not have any special limitation on the ultrasonic process. It can be carried out using a process well known to those skilled in the art and ensuring uniform mixing.
[0067] In the present invention, the mass concentration of g-C3N4-SO3H in the casting solution is preferably 0 to 0.4%, and is not 0, more preferably 0.2 to 0.4%, and most preferably 0.3 to 0.4%.
[0068] After obtaining the casting solution, the present invention forms a film from the casting solution, and then boils it in a hydrogen peroxide solution, a sulfuric acid solution and water in sequence to obtain a g-C3N4-SO3H / Nafion membrane.
[0069] In the present invention, the film forming process is preferably to pour the casting liquid into a polytetrafluoroethylene mold with grooves and sequentially perform first drying, second drying and cooling. In the present invention, the temperature of the first drying is preferably 293-403K, more preferably 313-383K, most preferably 333-363K, and the time is preferably 0.5-6h, more preferably 1-5h, and most preferably 1.5-4h; the temperature of the second drying is preferably 333-433K, more preferably 353-413K, most preferably 363-403K, and the time is preferably 0.1-5h, more preferably 0.4-4h, and most preferably 0.6-3h; the second drying method is preferably drying. The present invention does not have any special restrictions on the cooling process, and the process familiar to those skilled in the art can be used to cool to room temperature.
[0070] In the present invention, the mass concentration of the hydrogen peroxide solution is preferably 0.3-15%, more preferably 0.8-8%, and most preferably 1-6wt%; the boiling time in the hydrogen peroxide solution is preferably 0.1-8h, more preferably 0.4-5h, and most preferably 0.8-3h. In the present invention, the role of boiling in the hydrogen peroxide solution is to activate the Nafion membrane.
[0071] In the present invention, the concentration of the sulfuric acid solution is preferably 0.05-6 mol / L, more preferably 0.1-4 mol / L, and most preferably 0.2-2 mol / L; the boiling time in the sulfuric acid solution is preferably 0.1-8 h, more preferably 0.4-5 h, and most preferably 0.8-3 h. In the present invention, the role of boiling in the sulfuric acid solution is to activate the Nafion membrane.
[0072] In the present invention, the water is preferably deionized water. The boiling time in the water is preferably 0.1 to 8 hours, more preferably 0.4 to 5 hours, and most preferably 0.8 to 3 hours.
[0073] After obtaining the g-C3N4-SO3H / Nafion membrane, the present invention soaks the g-C3N4-SO3H / Nafion membrane in a soluble platinum salt solution, and then adds a sodium borohydride aqueous solution to obtain the membrane electrode.
[0074] Before the immersion, the present invention also preferably includes cutting the g-C3N4-SO3H / Nafion membrane. The present invention does not have any special limitation on the cutting process, and the cutting process may be carried out using a process well known to those skilled in the art.
[0075] In the present invention, the soluble platinum salt in the soluble platinum salt solution includes one or more of dichlorotetraammineplatinum, dichloroplatinum, tetrachloroplatinum, chloroplatinic acid and potassium chloroplatinate; when the soluble platinum salt is two or more of the above specific selections, the present invention does not have any special restrictions on the ratio of the above specific substances, and they can be mixed in any ratio. In the present invention, the concentration of the soluble platinum salt solution is preferably 0 to 1 mmol / L, and is not 0, more preferably 0.25 to 1 mmol / L, and most preferably 0.5 to 1 mmol / L;
[0076] In the present invention, the immersion temperature is preferably 293-353K, more preferably 303-393K, further preferably 313-363K, and most preferably 323-353K; the immersion time is preferably 0.5-36h, more preferably 1-48h, further preferably 5-36h, and most preferably 12-30h.
[0077] After the soaking is completed, the present invention preferably further comprises cleaning; the cleaning is preferably carried out using deionized water. The present invention does not have any special limitation on the cleaning process, and the cleaning process may be carried out using a process well known to those skilled in the art.
[0078] In the present invention, the mass percentage concentration of the sodium borohydride aqueous solution is preferably 0.1-10%, more preferably 0.05-8%, further preferably 0.2-5%, and most preferably 0.5-4%. In the present invention, the addition rate of the sodium borohydride aqueous solution is preferably 0.5-5 mL / min, more preferably 1-4 mL / min, and most preferably 1.5-3 mL / min. In the present invention, the process of adding the sodium borohydride aqueous solution is preferably carried out under the condition of 298K. In the present invention, each piece is 1.5*1.5 cm in size. 2 The amount of sodium borohydride aqueous solution used for the g-C3N4-SO3H / Nafion membrane is preferably 0.05 to 20 mL, more preferably 0.5 to 15 mL, and most preferably 1 to 12 mL.
[0079] The present invention also provides the application of the membrane electrode described in the above technical solution or the membrane electrode prepared by the preparation method described in the above technical solution in a fuel cell. The present invention has no special limitation on the application method, and the application method can be carried out by methods well known to those skilled in the art.
[0080] The membrane electrode and its preparation method and application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0081] Example 1
[0082] 100 mg of g-C3N4 was dispersed in 50 mL of deionized water, ultrasonicated at a frequency of 1000 Hz for 1 h, 5 mL of 0.1 mol / L sulfuric acid solution was added, magnetic stirring was performed at 333 K (stirring speed was 100 rpm, time was 6 h), and evaporated to obtain g-C3N4-SO3H;
[0083] By cell crushing method, 25 mg of g-C3N4-SO3H was dispersed in dimethyl sulfoxide to obtain a g-C3N4-SO3H dispersion with a concentration of 2.5 g / L;
[0084] Add 0.35 mL of the 2.5 g / L g-C3N4-SO3H dispersion to 2.2 mL of 20 wt% Nafion solution, and perform ultrasonic treatment to obtain a casting solution (the mass percentage concentration of g-C3N4-SO3H is 0.2%).
[0085] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4-SO3H / Nafion-0.2 membrane;
[0086] The g-C3N4-SO3H / Nafion-0.2 membrane was cut into 1.5*1.5cm 2 The size of the membrane was placed in 5mL of 1mmol / L Pt(NH3)4Cl2 solution and soaked for 24h. After being washed with deionized water, 2mL of 1wt% NaBH4 aqueous solution was added at a rate of 1.5mL / min at 298K. Metal Pt nanoparticles gradually formed on the membrane surface to obtain an integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-1.
[0087] Figure 1 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-1 at 303K~353K and 100% relative humidity, Figure 1 It can be seen that the proton conductivity at 80° C. and 100% relative humidity is 11.5 mS / cm.
[0088] Example 2
[0089] 100 mg of g-C3N4 was dispersed in 50 mL of deionized water, ultrasonicated at a frequency of 2000 Hz for 1 h, 5 mL of 0.1 mol / L sulfuric acid solution was added, magnetic stirring was performed at 333 K, and evaporated to obtain g-C3N4-SO3H;
[0090] By cell crushing method, 25 mg of g-C3N4-SO3H was dispersed in dimethyl sulfoxide to obtain a g-C3N4-SO3H dispersion with a concentration of 2.5 g / L;
[0091] Add 0.525 mL of the 2.5 g / L g-C3N4-SO3H dispersion to 2.2 mL of 20 wt% Nafion solution, and perform ultrasonic treatment to obtain a casting solution (the mass percentage concentration of g-C3N4-SO3H is 0.3%).
[0092] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4-SO3H / Nafion-0.3 membrane;
[0093] The g-C3N4-SO3H / Nafion-0.3 membrane was cut into 1.5*1.5cm 2 The size of the membrane was placed in 5mL of 5mmol / L Pt(NH3)4Cl2 solution and soaked for 24h. After being washed with deionized water, 2mL of 1wt% NaBH4 aqueous solution was added at a rate of 1.5mL / min at 298K. Metallic Pt nanoparticles gradually formed on the membrane surface, and an integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.3-0.5 was obtained.
[0094] Figure 2 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.3-0.5 at 303K~353K and 100% relative humidity, Figure 2 It can be seen that the proton conductivity at 80° C. and 100% relative humidity is 4.2 mS / cm.
[0095] Example 3
[0096] 100 mg of g-C3N4 was dispersed in 50 mL of deionized water, ultrasonicated at a frequency of 1000 Hz for 1 h, 5 mL of 0.1 mol / L sulfuric acid solution was added, magnetic stirring was performed at 333 K, and evaporated to obtain g-C3N4-SO3H;
[0097] By cell crushing method, 25 mg of g-C3N4-SO3H was dispersed in dimethyl sulfoxide to obtain a g-C3N4-SO3H dispersion with a concentration of 2.5 g / L;
[0098] Add 0.35 mL of the 2.5 g / L g-C3N4-SO3H dispersion to 2.2 mL of 20 wt% Nafion solution, and perform ultrasonic treatment to obtain a casting solution (the mass percentage concentration of g-C3N4-SO3H is 0.2%).
[0099] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4-SO3H / Nafion-0.2 membrane;
[0100] The g-C3N4-SO3H / Nafion-0.2 membrane was cut into 1.5*1.5cm 2 The size of the membrane was placed in 5 mL of a 0.25 mmol / L Pt(NH3)4Cl2 solution and soaked for 24 h. After being washed with deionized water, 3.5 mL of a 1 wt% NaBH4 aqueous solution was added at a rate of 1.5 mL / min at 298 K. Metal Pt nanoparticles gradually formed on the membrane surface, and an integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-0.25 was obtained.
[0101] Figure 3 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.2-0.25 at 303K~353K and 100% relative humidity, Figure 3 It can be seen that the proton conductivity rate at 70° C. and 100% relative humidity is 18.4 mS / cm, and the proton conductivity rate at 80° C. and 100% relative humidity is 6.1 mS / cm.
[0102] Example 4
[0103] 100 mg of g-C3N4 was dispersed in 50 mL of deionized water, ultrasonicated at a frequency of 1000 Hz for 1 h, 5 mL of 0.1 mol / L sulfuric acid solution was added, magnetic stirring was performed at 333 K, and evaporated to obtain g-C3N4-SO3H;
[0104] By cell crushing method, 25 mg of g-C3N4-SO3H was dispersed in dimethyl sulfoxide to obtain a g-C3N4-SO3H dispersion with a concentration of 2.5 g / L;
[0105] Add 0.7 mL of the 2.5 g / L g-C3N4-SO3H dispersion to 2.2 mL of 20 wt% Nafion solution, and perform ultrasonic treatment to obtain a casting solution (the mass percentage concentration of g-C3N4-SO3H is 0.4%).
[0106] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4-SO3H / Nafion-0.4 membrane;
[0107] The g-C3N4-SO3H / Nafion-0.4 membrane was cut into 1.5*1.5cm 2 The size of the membrane was placed in 5mL of 1mmol / L Pt(NH3)4Cl2 solution and soaked for 24h. After being washed with deionized water, 3.5mL of 1wt% NaBH4 aqueous solution was added at a rate of 1.5mL / min at 298K. Metal Pt nanoparticles gradually formed on the membrane surface to obtain an integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-1.
[0108] Figure 4 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-1 at 303K~353K and 100% relative humidity, Figure 4 It can be seen that the proton conductivity at 80° C. and 100% relative humidity is 3.2 mS / cm.
[0109] Example 5
[0110] 100 mg of g-C3N4 was dispersed in 50 mL of deionized water, ultrasonicated at a frequency of 1500 Hz for 1 h, 5 mL of 0.1 mol / L sulfuric acid solution was added, magnetic stirring was performed at 333 K, and evaporation was performed to obtain g-C3N4-SO3H;
[0111] By cell crushing method, 25 mg of g-C3N4-SO3H was dispersed in dimethyl sulfoxide to obtain a g-C3N4-SO3H dispersion with a concentration of 2.5 g / L;
[0112] Add 0.7 mL of the 2.5 g / L g-C3N4-SO3H dispersion to 2.2 mL of 20 wt% Nafion solution, and perform ultrasonic treatment to obtain a casting solution (the mass percentage concentration of g-C3N4-SO3H is 0.4%).
[0113] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4-SO3H / Nafion-0.4 membrane;
[0114] The g-C3N4-SO3H / Nafion-0.4 membrane was cut into 1.5*1.5cm 2 The size of the membrane was placed in 5mL of 0.25mmol / L Pt(NH3)4Cl2 solution and soaked for 24h. After being washed with deionized water, 2mL of 1wt% NaBH4 aqueous solution was added at a rate of 1.5mL / min at 298K. Metallic Pt nanoparticles gradually formed on the membrane surface, and an integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-0.25 was obtained.
[0115] Figure 5 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4-SO3H / Nafion-0.4-0.25 at 303K~353K and 100% relative humidity, Figure 5 It can be seen that the proton conductivity at 80° C. and 100% relative humidity is 2.83 mS / cm.
[0116] Comparative Example 1
[0117] 2.2 mL of a 20 wt% Nafion solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353 K for 2 h, dried at 393 K for 1 h, cooled to room temperature, and the obtained membrane was boiled in a 3 wt% hydrogen peroxide solution, a 0.5 mol / L sulfuric acid solution, and deionized water for 1 h to obtain a Nafion membrane.
[0118] The Nafion membrane was cut into 1.5*1.5 cm 2After the size was adjusted, it was placed in 5 mL of 0.25 mmol / L Pt(NH3)4Cl2 solution and immersed for 24 h. After being washed with deionized water, 2 mL of 1 wt% NaBH4 aqueous solution was added at a rate of 1.5 mL / min at 298 K. Metallic Pt nanoparticles gradually formed on the membrane surface, and an integrated membrane electrode of Pt@Nafion-1 was obtained.
[0119] Figure 6 is the proton conductivity curve of the integrated membrane electrode of Pt@Nafion-1 at 303K~353K and 100% relative humidity, Figure 6 It can be seen that the proton conductivity at 80° C. and 100% relative humidity is 2.1 mS / cm.
[0120] Comparative Example 2
[0121] 0.7 mL of the 2.5 g / L g-C3N4 dimethyl sulfoxide solution was added to 2.2 mL of the 20 wt% Nafion solution, and ultrasonicated to obtain a casting solution (the mass percentage concentration of g-C3N4 was 0.4%);
[0122] The casting solution was poured into a polytetrafluoroethylene mold with a groove, dried at 353K for 2 hours, dried at 393K for 1 hour, cooled to room temperature, and boiled in a 3wt% hydrogen peroxide solution, a 0.5mol / L sulfuric acid solution and deionized water for 1 hour to obtain a g-C3N4 / Nafion-0.4 membrane;
[0123] The g-C3N4 / Nafion-0.4 membrane was cut into 1.5*1.5 cm 2 The size of the membrane was placed in 5mL of 1mmol / L Pt(NH3)4Cl2 solution and soaked for 24h. After being washed with deionized water, 2mL of 1wt% NaBH4 aqueous solution was added at a rate of 1.5mL / min at 298K. Metal Pt nanoparticles gradually formed on the membrane surface to obtain an integrated membrane electrode of Pt@C3N4 / Nafion-0.4-1.
[0124] Figure 7 is the proton conductivity curve of the integrated membrane electrode of Pt@C3N4 / Nafion-0.4-1 at 303K~353K and 100% relative humidity, Figure 5 It can be seen that the proton conductivity at 80°C and 100% relative humidity is 1.6 mS / cm
[0125] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A membrane electrode, characterized in that: It comprises a modified Nafion membrane and Pt located on the surface of the modified Nafion membrane; The modified Nafion membrane is a g-C3N4-SO3H-doped Nafion membrane; The g-C3N4-SO3H in the modified Nafion membrane is g-C3N4 with -SO3H surface modification; The membrane electrode does not contain any binder.
2. The membrane electrode according to claim 1, characterized in that The mass percentage of g-C3N4-SO3H in the membrane electrode is 0 to 10%, and is not 0.
3. The membrane electrode according to claim 1 or 2, characterized in that: The mass of Pt in the membrane electrode is 0.05 to 1.5 mg per square centimeter.
4. The method for preparing a membrane electrode according to any one of claims 1 to 3, characterized in that: The following steps are involved: Sulfuric acid is added to the dispersion of g-C3N4 to modify it and obtain g-C3N4-SO3H; Mixing the g-C3N4-SO3H and an organic solvent to obtain a dispersion of g-C3N4-SO3H; Mixing the Nafion solution and the dispersion of g-C3N4-SO3H to obtain a film casting solution; After the casting solution is formed into a film, it is boiled in a hydrogen peroxide solution, a sulfuric acid solution and water in sequence to obtain a g-C3N4-SO3H / Nafion membrane; After the g-C3N4-SO3H / Nafion membrane is immersed in a soluble platinum salt solution, a sodium borohydride aqueous solution is added to obtain the membrane electrode.
5. The preparation method according to claim 4, characterized in that: The concentration of the g-C3N4 dispersion is 0.1 to 10 g / L; The concentration of the sulfuric acid is 0.01 to 5 mol / L; The volume ratio of the g-C3N4 dispersion and sulfuric acid is (0.1-50):
1.
6. The preparation method according to claim 4, characterized in that: The modification is carried out under stirring conditions; The stirring temperature is 293-363K, the rotation speed is 10-800 rpm, and the time is 3-24 hours.
7. The preparation method according to claim 4, characterized in that: The organic solvent includes one or more of dimethyl sulfoxide, cyclohexane, N,N-dimethylformamide, toluene, ethanol and methanol; The concentration of the g-C3N4-SO3H dispersion is 0.1 to 15 g / L.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The mass concentration of g-C3N4-SO3H in the casting solution is 0 to 0.4%, and is not 0.
9. The preparation method according to claim 4, characterized in that: The soluble platinum salt in the soluble platinum salt solution includes one or more of dichlorotetraammineplatinum, dichloroplatinum, tetrachloroplatinum, chloroplatinic acid and potassium chloroplatinate; The concentration of the soluble platinum salt solution is 0 to 1 mmol / L, and is not 0; The mass percentage concentration of the sodium borohydride aqueous solution is 0.1-10%; The immersion temperature is 293-353K and the immersion time is 0.5-36h; The process of adding the sodium borohydride aqueous solution is carried out under the condition of 298K.
10. Use of the membrane electrode according to any one of claims 1 to 3 or the membrane electrode prepared by the preparation method according to any one of claims 4 to 9 in a fuel cell.