Modified graphite felt, preparation method thereof and iron-chromium flow battery

By attaching high-oxygen-rich graphene and nanometal particles to the graphite felt and synergistically modifying the graphite felt, the problems of poor redox activity and hydrogen evolution reaction in iron-chromium flow batteries are solved, and the efficiency and life of the battery are improved.

CN118738430APending Publication Date: 2024-10-01HUBEI ZHENHUA CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410799846.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The Cr2+/Cr3+ redox activity in iron-chromium flow batteries is poor and there is a hydrogen evolution side reaction problem, which limits its development.

Method used

By attaching highly oxygen-rich graphene and nanometal particles, including active metals and hydrogen evolution suppressing metals, to the graphite felt, they are synergistically modified to improve conductivity and electrochemical activity, and inhibit the hydrogen evolution reaction.

Benefits of technology

It significantly improves the Coulombic efficiency and energy efficiency of the iron-chromium flow battery, reduces the battery's capacity fading rate, and extends the battery's cycle times and life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738430A_ABST
    Figure CN118738430A_ABST
Patent Text Reader

Abstract

The invention relates to a modified graphite felt, a preparation method thereof and an iron-chromium flow battery, the modified graphite felt comprises a graphite felt substrate, high oxygen-enriched graphene is attached to the graphite felt substrate, and nano metal particles are dispersed on the high oxygen-enriched graphene; the metal in the nano metal particles comprises an auxiliary active metal and a hydrogen evolution inhibiting metal. According to the preparation method disclosed by the invention, the conductivity and the electrochemical activity of the modified graphite felt are remarkably improved by virtue of mutual cooperation of an auxiliary active metal and a hydrogen evolution inhibiting metal in the nano metal particles and synergistic modification of the nano metal particles and the high oxygen-enriched graphene on the graphite felt; and meanwhile, the hydrogen evolution side reaction in the battery is effectively inhibited, so that the coulombic efficiency and the energy efficiency of the iron-chromium flow battery are improved, and the capacity fading rate of the battery is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of liquid flow batteries, and in particular to a modified graphite felt and a preparation method thereof, and an iron-chromium liquid flow battery. Background Art

[0002] Energy storage systems have the functions of power balancing, energy regulation, power stabilization, and ensuring stable power supply in the power grid. They are an important device to improve the quality of power grid electricity. With the implementation of the national strategy of "carbon peak and carbon neutrality", the direction for the future development of national energy has been clarified, and the high proportion of new energy grid connection has put forward an increasing demand for energy storage technology. Therefore, energy storage technology has an increasingly high status in my country's energy industry and has good development prospects.

[0003] Iron-chromium flow battery is a new type of flow battery that is cheap, efficient and environmentally friendly. Due to its advantages such as high specific energy and battery efficiency, simple and easy to control equipment, long life and low cost, it has a wide range of application prospects in power grid peak regulation, wind, electricity, solar and other new energy power generation. However, due to the Cr in iron-chromium flow battery 2+ / Cr 3+ The poor activity of the redox pair and the occurrence of hydrogen evolution side reaction during battery charging and discharging have also severely restricted the development of iron-chromium flow batteries.

[0004] As an important material for iron-chromium flow batteries, graphite felt electrodes have the advantages of good conductivity, strong corrosion resistance, and high temperature stability. However, the hydrophilicity of its surface and the electrochemical properties of the material itself cannot fully meet the needs of flow batteries, so it needs to be further activated and modified. By heat treating the graphite felt, adding active groups to its surface, and depositing catalysts on its surface, the surface morphology, chemical composition, and electrochemical properties of the graphite felt can be regulated, thereby effectively improving the electrical properties of the graphite felt.

[0005] CN116470071A discloses a method of modifying a graphite felt electrode using graphene oxide. The hydrophilicity and electrochemical activity of the modified graphite felt electrode are effectively improved, the polarization phenomenon of the electrode in an organic aqueous phase flow battery is weakened, and the capacity and efficiency of the battery are improved. However, the oxygen content of the graphene oxide modified on the graphite felt electrode is low, and the conductivity of the modified graphite felt electrode cannot meet the requirements of the flow battery. Moreover, the activity of the modified graphite felt electrode obtained by only modifying the graphene oxide cannot meet the requirements of the iron-chromium flow battery, and the occurrence of the hydrogen evolution reaction of the battery cannot be effectively suppressed.

[0006] Therefore, providing a modified graphite felt material that can not only simultaneously improve the conductivity and activity of the iron-chromium liquid flow battery electrode, but also effectively inhibit the occurrence of the hydrogen evolution reaction has become an urgent problem to be solved. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a modified graphite felt and a preparation method thereof and an iron-chromium liquid flow battery. The present invention significantly improves the conductivity and electrochemical activity of the modified graphite felt through the mutual coordination of the active metal and the hydrogen evolution inhibiting metal in the nanometal particles, and the synergistic modification of the graphite felt by the nanometal particles and the highly oxygen-rich graphene, and also effectively inhibits the occurrence of the hydrogen evolution side reaction in the battery, thereby improving the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery, and reducing the capacity attenuation rate of the battery.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a modified graphite felt, comprising a graphite felt substrate, to which high-oxygen-rich graphene is attached, and on which nano-metal particles are dispersed; the metal in the nano-metal particles comprises an active metal and a hydrogen evolution inhibiting metal.

[0010] The highly oxygen-rich graphene in the modified graphite felt provided by the present invention has abundant oxygen-containing functional groups and high hydrophilicity, can be well attached to the graphite felt substrate, and its abundant oxygen-containing functional groups can significantly improve the electrical conductivity of the graphite felt material; on the other hand, the highly oxygen-rich graphene can also be used as a carrier medium to provide more active sites, which is conducive to the dispersion of a large number of nano-metal particles on the highly oxygen-rich graphene, thereby realizing the introduction of nano-metal particles into the modified graphite felt.

[0011] In the nano-metal particles of the present invention, the auxiliary active metal can significantly improve the activity and stability of chromium in the iron-chromium liquid flow battery, but at the same time, the auxiliary active metal will also increase the activity of hydrogen in the battery, making the battery prone to hydrogen evolution side reactions during charging and discharging. Therefore, the present invention simultaneously introduces hydrogen evolution inhibitory metals into the modified graphite felt to effectively reduce the hydrogen evolution reaction in the iron-chromium liquid flow battery, thereby reducing the battery attenuation rate and extending the battery cycle times and life.

[0012] The present invention achieves significant improvement in the conductivity and electrochemical activity of the modified graphite felt by the mutual coordination of the active metal and the hydrogen evolution inhibiting metal in the nanometal particles and the synergistic modification of the graphite felt by the nanometal particles and the highly oxygen-rich graphene, while also effectively inhibiting the occurrence of the hydrogen evolution side reaction in the battery, thereby improving the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery and reducing the capacity attenuation rate of the battery.

[0013] Preferably, the auxiliary active metal includes any one of bismuth, tin, cerium or cobalt, or a combination of at least two of them.

[0014] Preferably, the hydrogen evolution inhibiting metal includes any one of lead, indium, zinc or tin, or a combination of at least two of them.

[0015] In the present invention, bismuth, tin, cerium or cobalt is selected as the auxiliary active metal. These metals and chromium element can reduce the electrochemical polarization effect, and can improve the electrocatalytic activity of the redox reaction of chromium and significantly improve the reversibility of the reaction, thereby improving the activity and stability of chromium in the iron-chromium liquid flow battery; at the same time, lead, indium, zinc or tin is selected as the hydrogen evolution inhibition metal. These metals have the function of hindering the kinetic process of hydrogen evolution reaction on the carbon surface and can inhibit the occurrence of hydrogen evolution side reaction in the battery. The mutual cooperation of the two can improve the activity of chromium without generating hydrogen evolution reaction, and jointly improve the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery, and reduce the capacity decay rate of the battery.

[0016] Preferably, the mass ratio of the auxiliary active metal to the hydrogen evolution inhibiting metal is (1-10):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1.

[0017] In the present invention, if the mass ratio is too large, the content of the hydrogen evolution inhibiting metal is too low, and the battery hydrogen evolution inhibiting effect is poor; if the mass ratio is too small, the content of the auxiliary active metal is too low, and the battery performance cannot be effectively improved.

[0018] Preferably, the particle size of the nano metal particles is 50-120 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm or 120 nm.

[0019] In the present invention, if the particle size of the nano metal particles is too large, they are easy to block the pores after being attached to the graphite felt, resulting in a decrease in the conductivity; if the particle size of the nano metal particles is too small, the attachment efficiency is low and the modification effect is poor.

[0020] Preferably, the ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :(0.05-0.5)mg:(1-20)mg, wherein the selection range of high oxygen-rich graphene is "(0.05-0.5)mg", for example, it can be 0.05mg, 0.06mg, 0.07mg, 0.08mg, 0.09mg, 0.1mg, 0.2mg, 0.3mg, 0.4mg or 0.5mg, etc.; the selection range of nanometal particles is "(1-20)mg", for example, it can be 1mg, 5mg, 10mg, 15mg or 20mg, etc.

[0021] Preferably, in the modified graphite felt described in the present invention, the mass ratio of the high oxygen-enriched graphene to the nano-metal particles is 1:25-150, for example, 1:25, 1:30, 1:50, 1:70, 1:90, 1:110, 1:130 or 1:150, etc.

[0022] In the present invention, if the content of highly oxygen-rich graphene is too little and the content of nano-metal particles is too much, the sites provided by the highly oxygen-rich graphene on the graphite felt are insufficient, which is not conducive to the attachment of nano-metal particles. In addition, the low content of highly oxygen-rich graphene will reduce the overall conductivity of the modified graphite felt, thereby affecting the electrochemical performance of the battery; if the content of highly oxygen-rich graphene is too much and the content of nano-metal particles is too little, the overall performance of the graphite felt will be slightly improved.

[0023] Preferably, the graphite felt substrate is connected to the high-oxygen-rich graphene via hydrogen bonds or van der Waals forces.

[0024] Preferably, the oxygen content in the highly oxygen-rich graphene is 38.5-40%, for example, 38.5%, 38.7%, 38.9%, 39.1%, 39.3%, 39.5%, 39.7%, 39.9% or 40%, etc.

[0025] In the present invention, "the oxygen content in the highly oxygen-rich graphene is 38.5-40%" means that the atomic ratio of oxygen atoms to carbon atoms in the highly oxygen-rich graphene is 38.5-40%.

[0026] In the present invention, if the oxygen content in the highly oxygen-rich graphene is low, the conductivity of the modified graphite felt will decrease, thereby causing the efficiency of the iron-chromium liquid flow battery to deteriorate.

[0027] In a second aspect, the present invention provides a method for preparing the modified graphite felt as described in the first aspect, the preparation method comprising the following steps:

[0028] (1) mixing a highly oxygen-rich graphene dispersion, an active agent, a hydrogen evolution inhibitor, an acid reagent, a reducing agent, and a solvent to obtain a graphite felt modified liquid;

[0029] (2) Immersing the heat-treated graphite felt into the graphite felt modification liquid obtained in step (1) to obtain the modified graphite felt through a hydrothermal reaction.

[0030] The present invention does not limit the order of adding materials in the "immersion" process. The heat-treated graphite felt can be added to the graphite felt modification liquid for immersion, or the graphite felt modification liquid can be added to the heat-treated graphite felt for immersion. Those skilled in the art can make the selection as needed.

[0031] The preparation method of the invention coordinates the metal ions in the high-oxygen-rich graphene with the rich functional groups on the surface of the high-oxygen-rich graphene and the active auxiliary agent and the hydrogen evolution inhibitor, so that the metal ions are dispersed in the high-oxygen-rich graphene, and then the added reducing agent reduces the metal ions into nano metal particles, so as to obtain the graphite felt modified liquid composed of nano metal particles including the active auxiliary metal and the hydrogen evolution inhibitor metal dispersed in the high-oxygen-rich graphene, wherein the acid reagent used has the function of increasing the solubility of the metal ions and increasing the reaction pressure.

[0032] The present invention uses heat-treated graphite felt for modification treatment, so that the graphite felt has hydrophilicity. When immersed in a graphite felt modification liquid, it is beneficial for highly oxygen-rich graphene dispersed with nano-metal particles to better adhere to the graphite felt base material, thereby forming a modified graphite felt. Applying the modified graphite felt to an iron-chromium liquid flow battery can improve the battery conductivity and activity, and effectively inhibit the occurrence of hydrogen evolution reaction in the battery.

[0033] Compared with the solid phase loading method, the hydrothermal reaction adopted in the present invention can make the nano metal particles in the modified graphite felt loaded more evenly and with better consistency. Meanwhile, the hydrothermal method is more suitable for mass production, has good repeatability and higher efficiency.

[0034] The process flow for preparing the modified graphite felt provided by the invention is simple, low-cost and environmentally friendly.

[0035] Preferably, the steps of preparing the highly oxygen-rich graphene dispersion include:

[0036] Graphite is mixed with mixed acid to obtain a graphite dispersion, and the graphite dispersion is subjected to oxidation treatment and separation and washing to obtain the highly oxygen-rich graphene dispersion.

[0037] Preferably, the graphite comprises flaky graphite.

[0038] Preferably, the particle size of the scaly graphite is 800-1500 mesh, for example, 800 mesh, 900 mesh, 1000 mesh, 1100 mesh, 1200 mesh, 1300 mesh, 1400 mesh or 1500 mesh.

[0039] Preferably, the mixed acid comprises a combination of at least two of concentrated sulfuric acid, concentrated phosphoric acid or concentrated nitric acid, wherein typical but non-limiting combinations include a combination of concentrated sulfuric acid and concentrated nitric acid, a combination of concentrated sulfuric acid and concentrated phosphoric acid, a combination of concentrated phosphoric acid and concentrated nitric acid, or a combination of concentrated sulfuric acid, concentrated phosphoric acid and concentrated nitric acid, etc.

[0040] The source of concentrated sulfuric acid, concentrated phosphoric acid or concentrated nitric acid in the mixed acid of the present invention can be commercially available products.

[0041] Preferably, the mixing is performed in an ice water bath.

[0042] Preferably, the mixing method includes stirring.

[0043] Preferably, the stirring speed is 20-200 rpm, for example, 20 rpm, 40 rpm, 60 rpm, 80 rpm, 100 rpm, 120 rpm, 140 rpm, 160 rpm, 180 rpm or 200 rpm, etc.

[0044] Preferably, the mixing time is 0.5-2 h, such as 0.5 h, 1 h, 1.5 h or 2 h.

[0045] In one embodiment, the specific steps of preparing the highly oxygen-rich graphene dispersion include:

[0046] The graphite dispersion is mixed with potassium permanganate to obtain a mixed solution, and a hydrogen peroxide solution and a solvent are added to the mixed solution to obtain a mother solution. The mother solution is centrifuged and washed to obtain the high-oxygen-rich graphene dispersion.

[0047] The present invention adopts a mixed acid system and potassium permanganate to jointly oxidize graphite, which is beneficial to increase the oxygen content of the obtained graphene oxide. Among them, the mixed acid system can not only improve the oxidation efficiency and promote the increase of the oxygen content of the obtained graphene oxide, but also effectively shorten the reaction time and accelerate the reaction process.

[0048] Preferably, in the process of preparing the mother liquor, the ratio of the graphite, mixed acid, potassium permanganate, hydrogen peroxide and solvent used is 1g:(80-150)mL:(1-6)g:(1-6)mL:(20-100)mL, wherein the selection range of the mixed acid is "(80-150)mL", for example, it can be 80mL, 90mL, 100mL, 110mL, 120mL, 130mL, 140mL or 150mL, etc.; the selection range of potassium permanganate is "(1-6)g", for example, it can be 1g, 2g, 3g, 4g, 5g or 6g, etc.; the selection range of hydrogen peroxide is "(1-6)mL", for example, it can be 1mL, 2mL, 3mL, 4mL, 5mL or 6mL, etc.; the selection range of the solvent is "(20-100)mL", for example, it can be 20mL, 40mL, 60mL, 80mL or 100mL, etc.

[0049] In the process of preparing highly oxygen-enriched graphene, the present invention adjusts the ratio between graphite, mixed acid, potassium permanganate, hydrogen peroxide and solvent used in the mother liquor preparation process, which is conducive to the preparation of highly oxygen-enriched graphene, and increases the oxygen enrichment of the highly oxygen-enriched graphene and improves its performance.

[0050] Preferably, the centrifugal force of the centrifugal washing is 10000-24000N, for example, 10000N, 12000N, 14000N, 16000N, 18000N, 20000N, 22000N or 24000N.

[0051] Preferably, the centrifugation time for the centrifugal washing is 1-20 min, for example, 1 min, 3 min, 5 min, 7 min, 9 min, 11 min, 13 min, 15 min, 17 min, 19 min or 20 min, etc.

[0052] Preferably, in step (1), the mass ratio of the high oxygen-rich graphene dispersion to the active agent, the hydrogen evolution inhibitor, the acid reagent and the reducing agent is 1:40-100:5-40:20-300:40-400.

[0053] The present invention adjusts the mass ratio of the high-oxygen-rich graphene dispersion to the active auxiliary agent, the hydrogen evolution inhibitor, the acid reagent and the reducing agent within the above preferred range, which can effectively improve the conductivity, activity and hydrogen evolution inhibition of the modified graphite felt.

[0054] Preferably, the active auxiliary agent in step (1) includes any one or a combination of at least two of bismuth chloride, tin chloride, cerium chloride, cobalt chloride, bismuth nitrate, tin nitrate, cerium nitrate or cobalt nitrate.

[0055] Preferably, the hydrogen evolution inhibitor in step (1) comprises any one of lead chloride, indium chloride, zinc chloride, tin chloride, lead nitrate, indium nitrate, zinc nitrate or tin nitrate, or a combination of at least two thereof.

[0056] Preferably, the acid reagent in step (1) comprises any one of nitric acid, sulfuric acid, phosphoric acid or silicic acid, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of nitric acid and sulfuric acid, a combination of nitric acid and phosphoric acid, a combination of nitric acid and silicic acid, a combination of sulfuric acid and phosphoric acid, a combination of sulfuric acid and silicic acid, a combination of nitric acid, sulfuric acid and phosphoric acid, or a combination of sulfuric acid, phosphoric acid and silicic acid, etc.

[0057] Preferably, the concentration of the acid reagent is 0-10wt% and does not include 0wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, etc.

[0058] Preferably, in step (1), the reducing agent includes a first reducing agent or a second reducing agent, and the reducing property of the first reducing agent is lower than that of the second reducing agent.

[0059] Preferably, the first reducing agent comprises any one of ascorbic acid, ethanol, ethylene glycol, citric acid, oxalic acid, tartaric acid or glucose, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of ascorbic acid and ethanol, a combination of ascorbic acid and ethylene glycol, a combination of ascorbic acid and citric acid, a combination of ascorbic acid and oxalic acid, a combination of ascorbic acid and tartaric acid, a combination of ascorbic acid and glucose, a combination of ethylene glycol and citric acid, a combination of ethylene glycol and oxalic acid, a combination of oxalic acid and tartaric acid, or a combination of oxalic acid and glucose, etc., preferably ascorbic acid.

[0060] Preferably, the second reducing agent comprises sodium borohydride.

[0061] Preferably, the concentration of the first reducing agent is 10-30wt%, for example 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt% or 30wt%, etc.

[0062] Preferably, the concentration of the second reducing agent is 1-10wt%, for example 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, etc.

[0063] The present invention adjusts the type and concentration of the reducing agent in step (1), that is, controls the reducibility of the solution within a stable range, and uses a reducing agent with relatively weak reducibility or a reducing agent with relatively low concentration, so as to ensure that the reducing agent reduces the metal ions in the active auxiliary agent and the hydrogen evolution inhibitor into metal element particles, but does not reduce the graphene oxide, thereby ensuring the successful preparation of the nano-metal particles and highly oxygen-rich graphene in the modified graphite felt. For example, using ascorbic acid as a reducing agent can reduce bismuth ions into bismuth element.

[0064] Preferably, the heat treatment in step (2) adopts a step-by-step heating method.

[0065] Preferably, the step-by-step temperature increase method includes a first step, a second step and a third step.

[0066] Preferably, the heating temperature of the first step is 50-100°C, such as 50°C, 60°C, 70°C, 80°C, 90°C or 100°C.

[0067] Preferably, the insulation time of the first step is 10-50 min, for example, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min or 50 min, etc.

[0068] Preferably, the heating temperature of the second step is 150-300°C, such as 150°C, 180°C, 210°C, 240°C, 270°C or 300°C.

[0069] Preferably, the insulation time of the second step is 30-100 min, for example, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min or 100 min, etc.

[0070] Preferably, the heating temperature of the third step is 300-500°C, for example, 300°C, 340°C, 380°C, 420°C, 460°C or 500°C.

[0071] Preferably, the insulation time of the third step is 300-400 min, for example, 300 min, 320 min, 340 min, 360 min, 380 min or 400 min.

[0072] Preferably, the pressure of the hydrothermal reaction in step (2) is 0.1-0.7 MPa, for example, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa or 0.7 MPa.

[0073] Preferably, the temperature of the hydrothermal reaction in step (2) is 130-170°C, such as 130°C, 140°C, 150°C, 160°C or 170°C.

[0074] Preferably, the hydrothermal reaction time in step (2) is 5-12 h, for example, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h.

[0075] Preferably, the product after the hydrothermal reaction in step (2) is further cooled, washed and dried.

[0076] In a third aspect, the present invention provides an iron-chromium liquid flow battery, wherein the iron-chromium liquid flow battery comprises the modified graphite felt as described in the first aspect.

[0077] The iron-chromium liquid flow battery provided by the present invention comprises modified graphite felt, wherein the mutual coordination of the active metal and the hydrogen evolution inhibiting metal in the nano-metal particles, and the synergistic effect of the nano-metal particles and the highly oxygen-rich graphene, make the conductivity and electrochemical activity of the modified graphite felt significantly improved, and also effectively inhibit the occurrence of the hydrogen evolution side reaction in the battery, thereby improving the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery, and reducing the capacity attenuation rate of the battery.

[0078] The present invention has no special requirements on other components of the iron-chromium liquid flow battery, and components commonly used by those skilled in the art may be used.

[0079] Compared with the prior art, the present invention has at least the following beneficial effects:

[0080] (1) In the modified graphite felt provided by the present invention, highly oxygen-rich graphene is attached to the graphite felt substrate, which can significantly improve the conductivity of the electrode material. The highly oxygen-rich graphene is used as a carrier of nano-metal particles. Nano-metal particles are introduced into the modified graphite felt. On the one hand, the auxiliary active metal in the nano-metal particles improves the activity and stability of chromium in the iron-chromium liquid flow battery. On the other hand, the hydrogen evolution inhibitory metal in the nano-metal particles effectively inhibits the occurrence of hydrogen evolution reaction in the iron-chromium liquid flow battery. The present invention significantly improves the conductivity and electrochemical activity of the modified graphite felt through the mutual coordination of the auxiliary active metal particles and the hydrogen evolution inhibitory metal in the nano-metal particles, and the synergistic modification of the graphite felt by the nano-metal particles and the highly oxygen-rich graphene, while also effectively inhibiting the occurrence of the hydrogen evolution side reaction in the battery.

[0081] (2) The preparation method of the modified graphite felt provided by the present invention uses heat-treated graphite felt for modification, so that the graphite felt has hydrophilicity, which is conducive to the better adhesion of highly oxygen-rich graphene dispersed with nano-metal particles on the graphite felt base material, thereby forming modified graphite felt to improve the conductivity and activity of the iron-chromium liquid flow battery, and effectively inhibit the occurrence of hydrogen evolution reaction in the battery. The process flow for preparing the modified graphite felt provided by the present invention is simple, low-cost, and green and environmentally friendly.

[0082] (3) The iron-chromium liquid flow battery provided by the present invention includes modified graphite felt, which effectively improves the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery and reduces the capacity attenuation rate of the battery, so that the iron-chromium liquid flow battery has excellent comprehensive electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] Figure 1 is a scanning electron microscope image of the untreated graphite felt in Example 1.

[0084] Figure 2 This is a scanning electron microscope image of the graphite felt after the heat treatment in Example 1.

[0085] Figure 3 is a scanning electron microscope image of the final modified graphite felt in Example 1.

[0086] Figure 4 The iron-chromium flow battery assembled with the modified graphite felt in Example 1 is 140 mA / cm 2 Cycling performance curve under current density.

[0087] Figure 5 The iron-chromium flow battery assembled with the modified graphite felt in Example 2 is 140 mA / cm2 Cycling performance curve under current density.

[0088] Figure 6 The iron-chromium flow battery assembled with the modified graphite felt in Example 3 is 140 mA / cm 2 Cycling performance curve under current density.

[0089] Figure 7 The iron-chromium liquid flow battery assembled with the modified graphite felt in Example 4 is 140 mA / cm 2 Cycling performance curve under current density.

[0090] Figure 8 The iron-chromium flow battery assembled with unmodified graphite felt in Example 1 at 140 mA / cm 2 Cycling performance curve under current density.

[0091] Fig. 9 The iron-chromium flow battery assembled with the unmodified graphite felt in Example 2 was tested at 140 mA / cm 2 Cycling performance curve under current density. DETAILED DESCRIPTION

[0092] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0093] The source of the scaly graphite used in the following examples is Nanjing Greifa Carbon Materials Co., Ltd. (800-1400 mesh), the graphite felt is PAN-based graphite felt (2.5 mm), which is sourced from Liaoyang Jingu Carbon Fiber Technology Co., Ltd., and the mixed acids involved in the following examples are all obtained by mixing commercially available concentrated acids according to a volume ratio. Specifically, the concentration of concentrated sulfuric acid is 98wt%, the concentration of concentrated phosphoric acid is 85wt%, and the concentration of concentrated nitric acid is 68wt%.

[0094] Example 1

[0095] This embodiment provides a modified graphite felt, including a graphite felt substrate, on which is attached a highly oxygen-rich graphene with an oxygen content of 40%, and on which are dispersed nano-metal particles, wherein the metals in the nano-metal particles include tin and lead. The ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.06mg:6mg, the mass ratio of tin and lead in the nano metal particles is 3:1, and the particle size distribution of the nano metal particles is 70-110nm.

[0096] The preparation method of the modified graphite felt provided in this example is as follows:

[0097] (I) 1 g of 1000 mesh scaly graphite was mixed with 100 mL of mixed acid (composed of concentrated sulfuric acid and concentrated phosphoric acid in a volume ratio of 9:1), and stirred at 100 rpm for 1 h in an ice-water bath to obtain a scaly graphite dispersion;

[0098] (II) adding 4 g of potassium permanganate to the scaly graphite dispersion, stirring for 1 h, then heating to 50° C. and stirring at this temperature, slowly adding 3 mL of 6% hydrogen peroxide dispersion after stirring, controlling the temperature of the solution to not exceed 5° C., then adding 80 mL of deionized water, stirring after the addition, and cooling to room temperature to obtain a mother liquor, placing the mother liquor in a centrifuge, centrifuging at a centrifugal force of 15000 N for 10 min, repeating the centrifugal washing several times until the supernatant is neutral and then stopping the washing to obtain a highly oxygen-rich graphene dispersion;

[0099] (III) mixing the highly oxygen-rich graphene dispersion with tin chloride, lead chloride, 5 wt% nitric acid and 15 wt% ascorbic acid in a mass ratio of 1:80:20:100:200 to prepare a graphite felt modified liquid;

[0100] (IV) Slice the graphite felt (the scanning electron microscope image is as follows) Figure 1 After that, the heat treatment was carried out at 75°C for 30 min, the temperature was raised to 220°C for 60 min, and the temperature was raised to 400°C for 350 min to obtain the heat-treated graphite felt (the scanning electron microscope image of which is shown in FIG. Figure 2 The treated graphite felt is then put into a reactor, and the graphite felt modification liquid obtained in step (III) is slowly added thereto. The modified graphite felt is subjected to a hydrothermal reaction at 150°C and 0.4 MPa for 10 h, and then cooled, washed and dried to obtain a modified graphite felt (the scanning electron microscope image of which is shown in FIG. Figure 3 shown).

[0101] Depend on Figure 1-Figure 3 It can be seen that Figure 1 Unmodified graphite felt and Figure 2 Compared with the morphology of the fibers in the heat-treated graphite felt, Figure 3 The fiber morphology of the modified graphite felt is smoother. This is because the highly oxygen-rich graphene is attached to the graphite felt, which can make the pits on the surface of the graphite felt smooth, and, Figure 3 The modified graphite felt in the present invention also has a large amount of granular substances, which correspond to the nano-metal particles dispersed on the surface of the highly oxygen-rich graphene.

[0102] This embodiment also provides an iron-chromium liquid flow battery consisting of a flow field frame, the above-mentioned modified graphite felt, a non-fluorocarbon-hydrogen porous membrane, a bipolar plate and a current collecting plate.

[0103] Example 2

[0104] This embodiment provides a modified graphite felt, including a graphite felt substrate, on which is attached a highly oxygen-rich graphene with an oxygen content of 40%, and on which are dispersed nano-metal particles, wherein the metals in the nano-metal particles include bismuth and lead. The ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.1mg:10mg, the mass ratio of bismuth and lead in the nano metal particles is 5:1, and the particle size distribution of the nano metal particles is 70-110nm.

[0105] The preparation method of the modified graphite felt provided in this example is as follows:

[0106] (I) 1 g of 800 mesh scaly graphite was mixed with 120 mL of mixed acid (composed of concentrated sulfuric acid and concentrated phosphoric acid in a volume ratio of 8:2), and stirred at 50 rpm for 2 h in an ice-water bath to obtain a scaly graphite dispersion;

[0107] (II) adding 5 g of potassium permanganate to the scaly graphite dispersion, stirring for 1 hour, then heating to 50° C. and stirring at this temperature, slowly adding 5 mL of 6% hydrogen peroxide dispersion after stirring, controlling the temperature of the solution to not exceed 5° C., then adding 100 mL of deionized water, stirring after the addition, and cooling to room temperature to obtain a mother liquor, placing the mother liquor in a centrifuge, centrifuging at a centrifugal force of 10,000 N for 20 minutes, repeating the centrifugal washing several times until the supernatant is neutral and then stopping the washing to obtain a highly oxygen-rich graphene dispersion;

[0108] (III) mixing the high oxygen-rich graphene dispersion with bismuth chloride, lead chloride, 2 wt% sulfuric acid and 12 wt% citric acid in a mass ratio of 1:80:20:250:160 to prepare a graphite felt modified liquid;

[0109] (IV) After the graphite felt is sliced, it is kept at 50°C for 50 minutes, heated to 280°C for 50 minutes, and then heated to 320°C for 390 minutes to obtain heat-treated graphite felt. The treated graphite felt is then put into a reactor, and the graphite felt modification liquid obtained in step (III) is slowly added thereto. A hydrothermal reaction is carried out at 130°C and 0.2 MPa for 12 hours, and then the modified graphite felt is obtained after cooling, washing and drying.

[0110] This embodiment also provides an iron-chromium liquid flow battery consisting of a flow field frame, the above-mentioned modified graphite felt, a non-fluorocarbon-hydrogen porous membrane, a bipolar plate and a current collecting plate.

[0111] Example 3

[0112] This embodiment provides a modified graphite felt, including a graphite felt substrate, on which is attached a highly oxygen-rich graphene with an oxygen content of 40%, and on which are dispersed nano-metal particles, wherein the metals in the nano-metal particles include bismuth and indium. The ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.05mg:5mg, the mass ratio of bismuth and indium in the nano metal particles is 7:1, and the particle size distribution of the nano metal particles is 70-110nm.

[0113] The preparation method of the modified graphite felt provided in this example is as follows:

[0114] (I) 1 g of 1400 mesh scaly graphite was mixed with 80 mL of mixed acid (composed of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 9:1), and stirred at 180 rpm for 0.6 h in an ice-water bath to obtain a scaly graphite dispersion;

[0115] (II) adding 3 g of potassium permanganate to the scaly graphite dispersion, stirring for 1 hour, then heating to 50° C. and stirring at this temperature, slowly adding 2 mL of 6% hydrogen peroxide dispersion after stirring, controlling the temperature of the solution to not exceed 5° C., then adding 60 mL of deionized water, stirring after the addition, and cooling to room temperature to obtain a mother liquor, placing the mother liquor in a centrifuge, centrifuging at a centrifugal force of 23000 N for 5 minutes, repeating the centrifugal washing several times until the supernatant is neutral and then stopping the washing to obtain a highly oxygen-rich graphene dispersion;

[0116] (III) mixing the highly oxygen-rich graphene dispersion with bismuth nitrate, indium nitrate, 7 wt % phosphoric acid and 25 wt % tartaric acid in a mass ratio of 1:80:20:70:75 to prepare a graphite felt modified liquid;

[0117] (IV) After the graphite felt is sliced, it is kept at 100°C for 20 minutes, heated to 160°C for 90 minutes, and then heated to 480°C for 300 minutes to obtain heat-treated graphite felt, and then the treated graphite felt is put into a reactor, and the graphite felt modification liquid obtained in step (III) is slowly added, and a hydrothermal reaction is carried out at 170°C and 0.5 MPa for 5 hours, and then after cooling, washing and drying, modified graphite felt is obtained.

[0118] This embodiment also provides an iron-chromium liquid flow battery consisting of a flow field frame, the above-mentioned modified graphite felt, a non-fluorocarbon-hydrogen porous membrane, a bipolar plate and a current collecting plate.

[0119] Example 4

[0120] This embodiment provides a modified graphite felt, including a graphite felt substrate, on which is attached a highly oxygen-rich graphene with an oxygen content of 40%, and on which are dispersed nano-metal particles, wherein the metals in the nano-metal particles include cerium and lead. The ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.06mg:8mg, the mass ratio of cerium and lead in the nano metal particles is 8:1, and the particle size distribution of the nano metal particles is 70-110nm.

[0121] The preparation method of the modified graphite felt provided in this example is as follows:

[0122] (I) 1 g of 900 mesh scaly graphite was mixed with 100 mL of mixed acid (composed of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 8:2), and stirred at 60 rpm for 1.8 h in an ice-water bath to obtain a scaly graphite dispersion;

[0123] (II) adding 4 g of potassium permanganate to the scaly graphite dispersion, stirring for 1 hour, then heating to 50° C. and stirring at this temperature, slowly adding 4 mL of 6% hydrogen peroxide dispersion after stirring, controlling the temperature of the solution to not exceed 5° C., then adding 90 mL of deionized water, stirring after the addition, and cooling to room temperature to obtain a mother liquor, placing the mother liquor in a centrifuge, centrifuging at a centrifugal force of 13000 N for 18 minutes, repeating the centrifugal washing several times until the supernatant is neutral and then stopping the washing to obtain a highly oxygen-rich graphene dispersion;

[0124] (III) mixing the high oxygen-rich graphene dispersion with cerium nitrate, indium nitrate, 8 wt% phosphosilicic acid and 5 wt% sodium borohydride in a mass ratio of 1:80:20:60:360 to prepare a graphite felt modified liquid;

[0125] (IV) After the graphite felt is sliced, it is kept at 60°C for 40 minutes, heated to 270°C and kept for 40 minutes, and then heated to 350°C and kept for 320 minutes to obtain heat-treated graphite felt, and then the treated graphite felt is put into a reactor, and the graphite felt modification liquid obtained in step (III) is slowly added, and a hydrothermal reaction is carried out at 140°C and 0.3 MPa for 10 hours, and then cooled, washed, and dried to obtain modified graphite felt.

[0126] This embodiment also provides an iron-chromium liquid flow battery consisting of a flow field frame, the above-mentioned modified graphite felt, a non-fluorocarbon-hydrogen porous membrane, a bipolar plate and a current collecting plate.

[0127] Example 5

[0128] The difference between this embodiment and embodiment 1 is that the metals in the nano metal particles in the modified graphite felt provided in this embodiment are copper and lead. The rest is the same as embodiment 1.

[0129] Example 6

[0130] The difference between this embodiment and embodiment 1 is that the metals in the nano metal particles in the modified graphite felt provided in this embodiment are tin and copper. The rest is the same as embodiment 1.

[0131] Example 7

[0132] The difference between this embodiment and embodiment 1 is that in the modified graphite felt provided in this embodiment, the ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.4mg:2mg, that is, the mass ratio of highly oxygen-rich graphene to nano-metal particles is 1:5. The rest is the same as in Example 1.

[0133] Example 8

[0134] The difference between this embodiment and embodiment 1 is that in the modified graphite felt provided in this embodiment, the ratio of the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :0.05mg:12mg, that is, the mass ratio of highly oxygen-rich graphene to nano-metal particles is 1:240. The rest is the same as in Example 1.

[0135] Example 9

[0136] The difference between this embodiment and embodiment 1 is that the mass ratio of tin to lead in the modified graphite felt provided in this embodiment is 0.5:1. The rest is the same as embodiment 1.

[0137] Example 10

[0138] The difference between this embodiment and embodiment 1 is that the mass ratio of tin to lead in the modified graphite felt provided in this embodiment is 11:1. The rest is the same as embodiment 1.

[0139] Embodiment 11

[0140] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified graphite felt provided in this embodiment, the amount of mixed acid added is 40 mL, and the oxygen content of the highly oxygen-rich graphene in the obtained modified graphite felt is 38.4%. The rest is the same as embodiment 1.

[0141] Example 12

[0142] The difference between this embodiment and embodiment 1 is that in the preparation method of the modified graphite felt provided in this embodiment, the acid mixed with the flaky graphite is only concentrated sulfuric acid, and the oxygen content of the highly oxygen-rich graphene in the obtained modified graphite felt is 38.3%. The rest is the same as embodiment 1.

[0143] Comparative Example 1

[0144] The difference between this comparative example and Example 1 is that the modified graphite felt provided in this comparative example uses the same batch of unmodified graphite felt as in Example 1, and no modification treatment is performed on the graphite felt. The rest is the same as in Example 1.

[0145] Comparative Example 2

[0146] The difference between this comparative example and Example 3 is that the modified graphite felt provided in this comparative example uses the same batch of unmodified graphite felt as in Example 3, and no modification treatment is performed on the graphite felt. The rest is the same as in Example 3.

[0147] Comparative Example 3

[0148] The difference between this comparative example and Example 1 is that in the modified graphite felt provided in this comparative example, the highly oxygen-rich graphene is replaced by commercially available graphene oxide. The rest is the same as Example 1.

[0149] Comparative Example 4

[0150] The difference between this comparative example and Example 1 is that in the modified graphite felt provided in this comparative example, the highly oxygen-rich graphene is omitted, and only nano-tin particles and nano-lead particles are used to modify the graphite felt. The rest is the same as Example 1.

[0151] Comparative Example 5

[0152] The difference between this comparative example and Example 1 is that in the modified graphite felt provided in this comparative example, nano metal particles are omitted and only highly oxygen-rich graphene is used to modify the graphite felt. The rest is the same as Example 1.

[0153] Test Method

[0154] The electrochemical performance of the iron-chromium flow battery provided in the above examples and comparative examples was tested at 140 mA / cm 2 The charge and discharge tests were carried out at 65°C and the charging voltage was 0.65-1.18V.

[0155] Table 1

[0156]

[0157]

[0158] The test results show that:

[0159] (1) It can be seen from Examples 1 to 4 that the present invention uses highly oxygen-rich graphene and nano-metal particles containing active metals and hydrogen evolution-inhibiting metals to synergistically modify graphite felt, so that the conductivity and electrochemical activity of the modified graphite felt are significantly improved, and the occurrence of hydrogen evolution side reactions is also suppressed, thereby effectively improving the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery, and reducing the capacity attenuation rate of the battery, so that the iron-chromium liquid flow battery has excellent comprehensive electrochemical performance.

[0160] Figure 4-7 This is a cycle performance curve of about 100 cycles. In order to see the trend clearly, Figure 4 , Figure 5 and Figure 7 The cycle performance curve diagram only shows part of the cycle number. Figure 4 From the cycle performance curve, it can be seen that the average discharge capacity attenuation rate of the battery assembled with the modified graphite felt of Example 1 is 0.17% / cycle, and the battery energy efficiency is 74%. Figure 5 From the cycle performance curve, it can be seen that the average discharge capacity attenuation rate of the battery assembled with the modified graphite felt of Example 2 is 0.37% / cycle, and the battery energy efficiency is 75%; Figure 6 From the cycle performance curve, it can be seen that the average discharge capacity attenuation rate of the battery assembled with the modified graphite felt of Example 3 is 0.14% / cycle, and the battery energy efficiency is 77%; Figure 7 It can be seen from the cycle performance curve that the average discharge capacity attenuation rate of the battery assembled with the modified graphite felt of Example 4 is 0.35% / cycle, and the battery energy efficiency is 80%.

[0161] (2) By comparing Example 1 with Examples 5 and 6, it can be seen that replacing tin as an auxiliary active metal in the modified graphite felt with copper will result in the inability to effectively improve the activity and stability of the battery electrode, the battery energy efficiency is poor, the battery capacity decay rate is high, and the coulombic efficiency is also reduced; replacing the hydrogen evolution inhibitory metal lead in the modified graphite felt with copper will fail to inhibit the occurrence of the hydrogen evolution side reaction of the iron-chromium liquid flow battery, the battery's coulombic efficiency and energy density are low, and the capacity decay rate becomes high.

[0162] (3) By comparing Example 1 with Examples 7 and 8, it can be seen that in the present invention, if the content of high-oxygen-rich graphene is too much and the content of nano-metal particles is too little, the overall performance of the graphite felt is slightly improved; if the content of high-oxygen-rich graphene is too little and the content of nano-metal particles is too much, the sites provided by the high-oxygen-rich graphene on the graphite felt are insufficient, which is not conducive to the attachment of nano-metal particles. In addition, the low content of high-oxygen-rich graphene will reduce the overall conductivity of the modified graphite felt, thereby affecting the electrochemical performance of the battery.

[0163] (4) By comparing Example 1 with Examples 9 and 10, it can be seen that the present invention improves energy efficiency and reduces capacity decay by adjusting the mass ratio of active-type nanometal particles to hydrogen evolution inhibiting nanometal particles. If the mass ratio is too small, the content of active-type metal particles is too low, and the battery performance cannot be effectively improved; if the mass ratio is too large, the content of hydrogen evolution inhibiting metal particles is too low, and the hydrogen evolution inhibiting effect of the battery is poor.

[0164] (5) By comparing Example 1 with Examples 11 and 12, it can be seen that if the content of the mixed acid added in the present invention is low, so that the mass ratio of scaly graphite to the mixed acid, potassium permanganate and hydrogen peroxide is not within the preferred range of the present invention, and if the mixed acid component is replaced by a single type of acid, the oxygen content of the high-oxygen-rich graphene will be low, resulting in a lower conductivity of the modified graphite felt, thereby causing a decrease in the electrochemical performance of the iron-chromium liquid flow battery.

[0165] (6) By comparing Example 1 with Comparative Example 1 and Example 3 with Comparative Example 2, it can be seen that if the graphite felt is not modified, the conductivity of the electrode will be low, the activity will be poor, and the battery will easily undergo hydrogen evolution reaction, resulting in poor electrochemical performance of the iron-chromium liquid flow battery.

[0166] Figure 8-9 This is a cycle performance curve of about 100 cycles. In order to see the trend clearly, Fig. 9 The cycle performance curve diagram only shows part of the cycle number. Figure 8 From the cycle performance curve, it can be seen that the average discharge capacity attenuation rate of the battery assembled with the unmodified graphite felt of Comparative Example 1 is 0.44% / cycle, and the battery energy efficiency is 69%; Fig. 9 It can be seen from the cycle performance curve that the average discharge capacity attenuation rate of the battery assembled with the unmodified graphite felt of Comparative Example 2 is 0.52% / cycle, and the battery energy efficiency is 70%.

[0167] (7) By comparing Example 1 with Comparative Examples 3-4, it can be seen that if the high-oxygen-rich graphene in the present invention is replaced with commercially available graphene oxide or high-oxygen-rich graphene is not used for modification, the electrical conductivity of the modified graphite felt obtained will be poor and cannot meet the required conductivity of the iron-chromium liquid flow battery, thereby causing a significant decrease in battery performance.

[0168] (8) By comparing Example 1 with Comparative Example 5, it can be seen that if only high-oxygen-rich graphene is used to modify the graphite felt in the present invention, and the modification of the nano-metal particles is omitted, the activity and stability of the chromium ions in the battery will be insufficient, and the hydrogen evolution reaction will be prone to occur, thereby causing the attenuation rate of the iron-chromium liquid flow battery to increase, and the energy efficiency and coulombic efficiency to decrease.

[0169] In summary, the present invention achieves significant improvement in the conductivity and electrochemical activity of the modified graphite felt through the mutual coordination of the active metal and the hydrogen evolution inhibiting metal in the nanometal particles, as well as the synergistic modification of the graphite felt by the nanometal particles and the highly oxygen-rich graphene, while also effectively inhibiting the occurrence of the hydrogen evolution side reaction in the battery, thereby improving the coulombic efficiency and energy efficiency of the iron-chromium liquid flow battery, and reducing the capacity decay rate of the battery.

[0170] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A modified graphite felt, It is characterized in that The modified graphite felt comprises a graphite felt substrate, on which highly oxygen-rich graphene is attached, and on which nano-metal particles are dispersed; the metal in the nano-metal particles comprises an activity-promoting metal and a hydrogen evolution-inhibiting metal.

2. The modified graphite felt according to claim 1, It is characterized in that The auxiliary active metal includes any one of bismuth, tin, cerium or cobalt, or a combination of at least two thereof; Preferably, the hydrogen evolution inhibiting metal includes any one of lead, indium, zinc or tin, or a combination of at least two thereof; Preferably, the mass ratio of the auxiliary active metal to the hydrogen evolution inhibiting metal is (1-10):1; Preferably, the particle size of the nano metal particles is 50-120 nm.

3. The modified graphite felt according to claim 1 or 2, It is characterized in that The ratio between the graphite felt substrate, the highly oxygen-rich graphene and the nano-metal particles is 1 cm 3 :(0.05-0.5)mg:(1-20)mg; Preferably, the mass ratio of the highly oxygen-rich graphene to the nano-metal particles is 1:25-150; Preferably, the oxygen content in the highly oxygen-rich graphene is 38.5-40%.

4. A method for preparing the modified graphite felt according to any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: (1) mixing a highly oxygen-rich graphene dispersion, an active agent, a hydrogen evolution inhibitor, an acid reagent, a reducing agent, and a solvent to obtain a graphite felt modified liquid; (2) Immersing the heat-treated graphite felt into the graphite felt modification liquid obtained in step (1), and subjecting the modified graphite felt to a hydrothermal reaction, thereby obtaining the modified graphite felt.

5. The preparation method according to claim 4, It is characterized in that The preparation steps of the high oxygen-rich graphene dispersion include: Mixing graphite with mixed acid to obtain a graphite dispersion, and subjecting the graphite dispersion to oxidation treatment and separation and washing to obtain the highly oxygen-rich graphene dispersion; Preferably, the graphite comprises flaky graphite; Preferably, the particle size of the scaly graphite is 800-1500 mesh; Preferably, the mixed acid comprises a combination of at least two of concentrated sulfuric acid, concentrated phosphoric acid or concentrated nitric acid; Preferably, the mixing is carried out under ice water bath conditions; Preferably, the mixing method includes stirring; Preferably, the stirring speed is 20-200 rpm; Preferably, the mixing time is 0.5-2h.

6. The preparation method according to claim 5, It is characterized in that The specific steps of preparing the high oxygen-rich graphene dispersion include: Mixing the graphite dispersion with potassium permanganate to obtain a mixed solution, adding a hydrogen peroxide solution and a solvent to the mixed solution to obtain a mother solution, and washing the mother solution by centrifugation to obtain the high-oxygen-rich graphene dispersion; Preferably, in the process of preparing the mother solution, the ratio of the graphite, mixed acid, potassium permanganate, hydrogen peroxide and solvent used is 1 g: (80-150) mL: (1-6) g: (1-6) mL: (20-100) mL; Preferably, the centrifugal force of the centrifugal washing is 10000-24000N; Preferably, the centrifugation time of the centrifugal washing is 1-20 min.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that In step (1), the mass ratio of the high oxygen-rich graphene dispersion to the active agent, the hydrogen evolution inhibitor, the acid reagent and the reducing agent is 1:40-100:5-40:20-300:40-400; Preferably, the active auxiliary agent in step (1) includes any one or a combination of at least two of bismuth chloride, tin chloride, cerium chloride, cobalt chloride, bismuth nitrate, tin nitrate, cerium nitrate or cobalt nitrate; Preferably, the hydrogen evolution inhibitor in step (1) comprises any one or a combination of at least two of lead chloride, indium chloride, zinc chloride, tin chloride, lead nitrate, indium nitrate, zinc nitrate or tin nitrate; Preferably, the acid reagent in step (1) comprises any one of nitric acid, sulfuric acid, phosphoric acid or silicic acid, or a combination of at least two thereof; Preferably, the concentration of the acid reagent is 0-10wt% and does not include 0wt%; Preferably, in step (1), the reducing agent includes a first reducing agent or a second reducing agent, and the reducing property of the first reducing agent is smaller than that of the second reducing agent; Preferably, the first reducing agent comprises any one or a combination of at least two of ascorbic acid, ethanol, ethylene glycol, citric acid, oxalic acid, tartaric acid or glucose, preferably ascorbic acid; Preferably, the second reducing agent comprises sodium borohydride; Preferably, the concentration of the first reducing agent is 10-30wt%; Preferably, the concentration of the second reducing agent is 1-10 wt %.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that The heat treatment in step (2) adopts a step-by-step temperature increase method; Preferably, the step-by-step heating method includes a first step, a second step and a third step; Preferably, the heating temperature of the first step is 50-100°C; Preferably, the insulation time of the first step is 10-50 min; Preferably, the heating temperature of the second step is 150-300°C; Preferably, the second step heat preservation time is 30-100min; Preferably, the heating temperature of the third step is 300-500°C; Preferably, the insulation time of the third step is 300-400 minutes.

9. The preparation method according to any one of claims 4 to 8, It is characterized in that The pressure of the hydrothermal reaction in step (2) is 0.1-0.7 MPa; Preferably, the temperature of the hydrothermal reaction in step (2) is 130-170°C; Preferably, the hydrothermal reaction time in step (2) is 5-12 hours; Preferably, the product after the hydrothermal reaction in step (2) is further cooled, washed and dried.

10. An iron-chromium flow battery, It is characterized in that The iron-chromium flow battery comprises the modified graphite felt as described in any one of claims 1-3.