Lithium battery and preparation method thereof
By mixing lithium iron phosphate or lithium iron manganese phosphate with carbon fluoride and ball milling in a lithium battery, a discharge reaction is performed to generate a carbon coating layer, which solves the problems of low performance of the cathode material of the lithium battery and insufficient binding force of the coating layer, and improves efficiency Battery cycle performance and stability.
Patent Information
- Application Number
- CN202411159129.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-01
AI Technical Summary
The existing lithium battery cathode material lithium iron phosphate (LMFP) has low electronic conductivity and lithium ion diffusion coefficient, resulting in limited performance at high rates. Moreover, the existing coating method is complex, costly, and has weak binding force, which can easily lead to The coating layer falls off, affecting battery performance and safety.
By mixing lithium iron phosphate or lithium iron manganese phosphate with carbon fluoride and ball milling, a discharge reaction is performed to generate a carbon coating layer, forming an in-situ carbon coating layer on the surface of the primary lithium battery to enhance the binding force with the cathode material.
It achieves uniform and firm coating of lithium iron phosphate or lithium manganese iron phosphate with carbon in the lithium battery, improves the cycle performance and stability of the battery, and reduces the risk of the coating layer falling off.
Smart Images

Figure CN118738515A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery preparation, and in particular to a lithium battery and a preparation method thereof. Background Art
[0002] Lithium batteries are widely used in various electronic devices and electric vehicles due to their high energy density, long cycle life and environmental protection. Among them, lithium iron phosphate (LMFP) is considered to be a promising lithium battery cathode material due to its high safety, low cost and environmental friendliness. However, LMFP has low electronic conductivity and lithium ion diffusion coefficient, which limits its performance at high rates. Some solutions are mainly to coat a layer of carbon material on the surface of LMFP to improve its electronic conductivity and lithium ion diffusion coefficient. This method mainly forms a carbon coating on the surface of LMFP by physical or chemical vapor deposition, sol-gel method and other methods. However, these methods often require high temperature treatment, and the bonding force between the coating and LMFP is weak, and it is easy to fall off during charging and discharging.
[0003] Although existing solutions have improved the performance of LMFP to a certain extent, there are still some problems. First, these methods usually require complex preparation processes and expensive equipment, which increases the manufacturing cost of the battery. Secondly, due to the weak bonding force between the coating layer and LMFP, the coating layer is easy to fall off during the charging and discharging process, which not only reduces the performance of the battery, but also may cause safety problems. In addition, the existing coating methods often cannot achieve uniform coating of LMFP, which may lead to inconsistent battery performance. Therefore, how to achieve uniform and firm coating of LMFP is an important challenge facing current battery manufacturing technology.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a lithium battery and a preparation method thereof, aiming to improve the carbon coating performance of lithium iron phosphate or lithium manganese iron phosphate in the lithium battery.
[0006] The present invention is achieved in that: In a first aspect, the present invention provides a method for preparing a lithium battery, comprising: Providing a preliminary lithium battery product, wherein the active material of the positive electrode sheet of the preliminary lithium battery product is a phosphate composite material, the phosphate composite material includes phosphate and carbon fluoride dispersed on the surface of the phosphate, the phosphate is selected from at least one of lithium iron phosphate and lithium manganese iron phosphate, and the electrolyte of the preliminary lithium battery product contains lithium ions; The initial lithium battery is discharged, and a finished lithium battery is obtained after the discharge is completed.
[0007] In an optional embodiment, the mass ratio of phosphate to carbon fluoride is 1:9~99.
[0008] In an optional embodiment, the mass ratio of phosphate to carbon fluoride is 1:29~99.
[0009] In an alternative embodiment, the chemical formula of the fluorinated carbon is CF x , where x is 1~2.
[0010] In an optional embodiment, the lithium battery is a button battery, the negative electrode material of the button battery is lithium, and the discharge conditions are: discharge to 2.5~3V at a current of 0.005~0.01C, and then discharge to 2.0~2.4V at 0.01C~0.02C; Alternatively, the discharge condition is: discharge to 2.0~2.4V at a current of 0.005~0.01C.
[0011] In an optional embodiment, the lithium battery is a full battery, the negative electrode material of the full battery is graphite, and the discharge conditions are: discharging to 0~0.1V with a current of 0.005~0.01C.
[0012] In an optional embodiment, the ambient temperature during discharge is 20-40°C.
[0013] In an optional embodiment, the preparation method of the lithium iron phosphate composite material includes: mixing lithium iron phosphate and carbon fluoride and ball milling them.
[0014] In an optional embodiment, the ball milling speed is 800-1000 rpm, and the ball milling time is 1-5 h.
[0015] In a second aspect, an embodiment of the present invention provides a lithium battery, which is prepared using the preparation method provided by the present invention.
[0016] The present invention has the following beneficial effects: In the method for preparing a lithium battery provided by an embodiment of the present invention, the prepared battery is first discharged, so that the carbon fluoride reacts to generate carbon coating on the surface of lithium iron phosphate or lithium iron manganese phosphate. The carbon coating layer generated by this in-situ reaction has a strong binding property with lithium iron phosphate or lithium iron manganese phosphate, and is not easy to fall off during the charge and discharge process of the battery. Therefore, the battery prepared by the preparation method provided by the present invention has good cycle performance because the surface of the lithium iron phosphate is coated with a coating layer with strong binding ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 It is a comparison chart of the cycle performance of some embodiments and comparative examples. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0020] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0021] An embodiment of the present invention provides a method for preparing a lithium battery, comprising: Providing a preliminary lithium battery product, wherein the active material of the positive electrode sheet of the preliminary lithium battery product is a phosphate composite material, the phosphate composite material includes phosphate and carbon fluoride dispersed on the surface of the phosphate, the phosphate is selected from at least one of lithium iron phosphate and lithium manganese iron phosphate, and the electrolyte of the preliminary lithium battery product contains lithium ions; The initial lithium battery is discharged, and a finished lithium battery is obtained after the discharge is completed.
[0022] In the method for preparing a lithium battery provided in an embodiment of the present invention, the prepared lithium battery is discharged, and the following reactions can occur during the discharge process: Li + +e-→Li; xLi+CF x →C+xLiF.
[0023] After the above reaction, a carbon coating layer can be generated in situ on the surface of lithium iron phosphate or lithium iron manganese phosphate. The carbon coating layer generated by the in situ reaction has a strong binding property with lithium iron phosphate or lithium iron manganese phosphate and is not easy to fall off during the charge and discharge process of the battery. Therefore, the battery prepared by the preparation method provided by the present invention has good cycle performance because the surface of the lithium iron phosphate is coated with a coating layer with strong binding ability.
[0024] The preparation method is specifically as follows: S1. Preparation of composite lithium iron phosphate composite materials At least one of lithium iron phosphate and lithium iron manganese phosphate is mixed with CFx The two materials are placed together in a ball mill, and ball milled for 1 to 5 hours (1 hour, 3 hours or 5 hours) at a ball milling speed of 800 to 1000 rpm (for example, 800 rpm, 900 rpm or 1000 rpm) to obtain a phosphate composite material.
[0025] Under the above ball milling conditions, CF x Stably and evenly loaded on the surface of lithium iron phosphate or lithium iron manganese phosphate.
[0026] Optionally, in order to make the battery have significantly better cycle performance, the mass ratio of lithium iron phosphate to carbon fluoride is 1:9-99 (eg, 1:9, 1:19, 1:39, 1:59, 1:79 or 1:99).
[0027] Furthermore, in order to make the battery have better cycle performance, the mass ratio of lithium iron phosphate to carbon fluoride is 1:29~99 (for example, 1:29, 1:39, 1:49, 1:59, 1:79 or 1:99).
[0028] Alternatively, the chemical formula of the carbon fluoride is CF x , where x is 1 to 2 (for example, 1, 1.1, 1.3, 1.5, 1.8, or 2).
[0029] S2. Obtaining initial lithium battery products The phosphate composite material is prepared into a primary lithium battery by a conventional preparation method, and the type of the lithium battery can be a button cell, a full cell, or other types of lithium batteries.
[0030] S2, discharge Optionally, when the lithium battery is a button battery, the negative electrode material of the button battery is lithium metal, and the discharge conditions are: 0.005~0.01C (for example, 0.005C, 0.008C or 0.01C) current discharge to 2.5~3V (for example, 2.5V, 2.8V or 3V), and then 0.01C~0.02C (for example, 0.01C, 0.015C or 0.02C) discharge to 2.0~2.4V (for example, 2.0V, 2.2V or 2.4V); Alternatively, the discharge condition is: discharging at a current of 0.005-0.01C (eg, 0.005C, 0.008C, or 0.01C) to a value of 2.0-2.4V (eg, 2.0V, 2.2V, or 2.4V).
[0031] When the lithium battery is a button cell, since the negative electrode is lithium metal, its voltage is relatively high, and it is discharged with a small current to 2.0~2.4V so that the carbon fluoride fully reacts to carbon.
[0032] Optionally, when the lithium battery is a full battery, the negative electrode material of the full battery is a carbon material, usually graphite, and the discharge conditions are: discharging at a current of 0.005~0.01C (such as 0.005C, 0.008C or 0.01C) to 0~0.1V (such as 0 V, 0.05V or 0.1V).
[0033] When the lithium battery is a full battery, since the negative electrode is graphite, its voltage is relatively low, and it is discharged with a small current to 0~0.1V, so that the carbon fluoride fully reacts into carbon.
[0034] Optionally, the ambient temperature during discharge is 20-40° C. (eg, 20° C., 30° C., or 40° C.).
[0035] The lithium battery provided in the embodiment of the present invention is prepared by the preparation method provided by the present invention. The battery has better cycle performance.
[0036] The present application is described in detail below in conjunction with a number of embodiments.
[0037] The lithium manganese iron phosphate used in the embodiment is LMFP64 from Tianjin Scholland, CFx is purchased from Aladdin's official website, and x is 2.
[0038] Example 1 The mass ratio of lithium manganese iron phosphate and CFx was 1:99, and they were mixed evenly by grinding at 800 rpm for 2 h in a ball mill to obtain a phosphate composite material.
[0039] The phosphate composite material is made into a positive electrode sheet. The specific preparation method is as follows: the phosphate composite material, SP and PVDF are added into a degassing machine according to a mass ratio of 90:50:5, and the stirring speed is 2000rpm to obtain a slurry, which is coated on a 12µm aluminum foil (the thickness of the carbon coating layer is 1µm) to obtain a positive electrode sheet.
[0040] The positive electrode sheet is assembled into a button battery. The specific assembly method is as follows: first roll the positive electrode sheet to a compaction density of 2.3g / cc, and bake the positive electrode sheet in a vacuum oven for 12 hours to ensure that the electrode sheet is dry; place the positive electrode shell flat on the workbench with the shell opening facing up, and use tweezers to place the positive electrode sheet at the bottom of the positive electrode shell to ensure that the positive electrode sheet is in full contact with the shell bottom. Use a pipette to absorb an appropriate amount of electrolyte and drip it onto the positive electrode sheet. Take a suitable diaphragm and carefully place it on the positive electrode sheet so that it completely covers the positive electrode sheet; use a pipette to absorb an appropriate amount of electrolyte and drip it onto the diaphragm to ensure that the electrolyte is evenly distributed; place the negative electrode sheet on the wet diaphragm, align the negative electrode shell with the positive electrode shell, and press gently to make the positive and negative electrode shells fit tightly. A special sealing machine can be used to seal the battery to ensure that the battery is well sealed to prevent electrolyte leakage.
[0041] The assembled button battery was discharged at 25°C, first using a constant current of 0.005C to 3.0V, and then 0.01C to 2.4V.
[0042] Embodiment 2~4 Examples 2 to 4 are substantially the same as Example 1, except that the mass ratios of lithium manganese iron phosphate and CFx are 1:49, 1:29, and 1:9, respectively.
[0043] Example 5 This embodiment is basically the same as Embodiment 1, except that: The assembled button battery was discharged at 25°C, first using a constant current of 0.008C to 2.5V, and then 0.015C to 2.2V.
[0044] Example 6 This embodiment is basically the same as Embodiment 1, except that: The assembled button battery was discharged at 25°C, first using a constant current of 0.01C to 2.8V, and then 0.02C to 2.0V.
[0045] Comparative Example 1 This comparative example is basically the same as Example 1, except that the positive electrode sheet is directly made of lithium manganese iron phosphate.
[0046] Comparative Example 2 This comparative example is basically the same as Example 1, except that the lithium battery is not discharged after being prepared.
[0047] Comparative Example 3 This comparative example is basically the same as Example 1, except that CFx is replaced by an equal amount of nano-scale carbon powder.
[0048] Experimental example The buckle batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were tested at 45 degrees by charging at 0.5C constant current to 4.5V, charging at 4.5V constant voltage to 0.05C, and discharging at 0.5C constant current to 2.0V, and cycled until the capacity decayed to 80%. The test results are recorded in Table 1 and Figure 1 middle.
[0049] Table 1 Cycle number records of some embodiments and comparative examples
[0050] From Table 1 and Figure 1 It can be seen that the batteries prepared in various embodiments of the present invention have a higher number of cycles, which is significantly higher than that of Comparative Example 1 and Comparative Example 2.
[0051] Comparing Comparative Example 1 with Example 1, the number of cycles of Comparative Example 1 is significantly lower, indicating that the combination of lithium manganese iron phosphate and carbon fluoride can significantly improve the cycle performance of the cycle battery.
[0052] Comparing Comparative Example 2 with Example 1, the number of cycles of Comparative Example 2 is significantly lower, indicating that the surface of the lithium manganese iron phosphate can be coated with a carbon layer through discharge treatment after the initial battery is made. If it is not discharged first, it is difficult to form a stable coating layer on the surface of the lithium manganese iron phosphate.
[0053] Comparing Comparative Example 3 with Example 1, the number of cycles of Comparative Example 3 is lower. In Comparative Example 3, carbon is directly coated on the surface of lithium iron manganese phosphate, rather than being in-situ grown on the surface of lithium iron manganese phosphate through discharge. This shows that the carbon coating layer formed on the surface of lithium iron manganese phosphate through discharge by the method provided by the present invention has better stability.
[0054] In summary, the preparation method of the lithium battery provided by the embodiment of the present invention is to discharge the prepared battery product first, so that the carbon fluoride reacts to generate carbon coating on the surface of lithium iron phosphate or lithium iron manganese phosphate. The carbon coating layer generated by this in-situ reaction has a strong binding property with lithium iron phosphate or lithium iron manganese phosphate, and is not easy to fall off during the charge and discharge process of the battery. Therefore, the battery prepared by the preparation method provided by the present invention has good cycle performance because the surface of the lithium iron phosphate is coated with a coating layer with strong binding ability.
[0055] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a lithium battery, characterized in that: include: Providing a preliminary lithium battery product, wherein the active material of the positive electrode sheet of the preliminary lithium battery product is a phosphate composite material, the phosphate composite material includes a phosphate and carbon fluoride dispersed on the surface of the phosphate, the phosphate is selected from at least one of lithium iron phosphate and lithium manganese iron phosphate, and the electrolyte of the preliminary lithium battery product contains lithium ions; The lithium battery product is discharged, and a lithium battery product is obtained after the discharge is completed.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the phosphate to the carbon fluoride is 1:9-99.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the phosphate to the carbon fluoride is 1:29-99.
4. The preparation method according to claim 1, characterized in that: The chemical formula of the carbon fluoride is CF x , where x is 1~2.
5. The preparation method according to claim 1, characterized in that: The lithium battery is a button battery, the negative electrode material of the button battery is lithium, and the discharge conditions are: discharge at a current of 0.005-0.01C to 2.5-3V, and then discharge at a current of 0.01C-0.02C to 2.0-2.4V; Alternatively, the discharge condition is: discharge to 2.0~2.4V at a current of 0.005~0.01C.
6. The preparation method according to claim 5, characterized in that: The lithium battery is a full battery, the negative electrode material of the full battery is graphite, and the discharge condition is: discharging at a current of 0.005~0.01C to 0~0.1V.
7. The preparation method according to claim 5, characterized in that: The ambient temperature during discharge is 20~40℃.
8. The preparation method according to claim 1, characterized in that: The preparation method of the lithium iron phosphate composite material comprises: mixing the lithium iron phosphate and the carbon fluoride and performing ball milling.
9. The preparation method according to claim 8, characterized in that: The ball milling speed is 800~1000rpm, and the ball milling time is 1~5h.
10. A lithium battery, characterized in that: The method is prepared according to any one of claims 1 to 9.