Low-temperature rate type lithium ion battery and preparation method thereof

By using the design of Li3xLa2/3-xTiO3-coated positive electrode and SnzLiy, LiTi2(PO4)3-coated negative electrode in lithium-ion batteries, the problem of poor high-rate charge and discharge performance of lithium-ion batteries at low temperatures is solved, and the problem of poor high-rate charge and discharge performance in low-temperature environments is achieved. high performance and long life.

CN118738522AInactive Publication Date: 2024-10-01JIANGSU OLITER ENERGY TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411079332.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium-ion batteries cannot achieve high-rate charging and discharging under low temperature conditions, resulting in reduced performance and shortened service life, which limits their application in fields such as electric vehicles and starting power supplies.

Method used

Li3xLa2/3-xTiO3 is used to coat the surface of lithium iron phosphate to form the positive active material, and SnzLiy and LiTi2(PO4)3 are coated on the hard carbon surface to form the negative active material. Combined with the specific electrolyte composition and separator design, it forms Low temperature rate lithium-ion battery.

Benefits of technology

It achieves good high-rate charge and discharge performance of lithium-ion batteries in low-temperature environments, improves the kinetic properties and conductive properties of ions, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738522A_ABST
    Figure CN118738522A_ABST
Patent Text Reader

Abstract

The invention relates to a low-temperature rate type lithium ion battery and a preparation method thereof. The lithium ion battery comprises a plurality of positive plates and a plurality of negative plates opposite to the positive plates, a positive electrode material on the surface of the positive plate comprises a positive electrode active substance formed by coating the surface of lithium iron phosphate with Li < 3x > La < 2 / 3-x > TiO3, and the value range of x is 0.1-0.3; a negative electrode material on the surface of the negative plate comprises a negative electrode active substance formed by coating at least one of SnzLiy and LiTi2 (PO4) 3 on the surface of hard carbon, the value range of z is 1-22, and the value range of y is 1-5. According to the present invention, the lithium ion battery can form the fast ion conduction channel by using the positive electrode active material so as to improve the dynamic performance of the ion, and the lithium ion battery has characteristics of good conductivity, high specific capacity and low overpotential at the high rate by using the negative electrode active material, and has low-temperature large-rate charge-discharge performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a low-temperature rate lithium ion battery and a preparation method thereof. Background Art

[0002] Temperature has an important impact on lithium-ion batteries. Too low a temperature will not only cause the performance of lithium-ion batteries to decline and fail to work properly, but charging at low temperatures will also cause lithium deposition at the negative electrode, causing the battery capacity to decline rapidly, and in extreme cases, even causing a short circuit between the positive and negative electrodes. The characteristics of lithium-ion power batteries are relatively significantly affected by ambient temperature. When the practical ambient temperature is low, its energy and power decline more seriously. If used at this temperature for a long time, its service life will be shortened.

[0003] In the existing technology, high-rate lithium-ion batteries have poor fast charging acceptance, short service life at high-rate charging and discharging, and cannot be discharged at high rates under low temperature conditions. This greatly limits the use efficiency and application environment of lithium-ion batteries, and seriously restricts their promotion and use in electric vehicles, starting power supplies and other fields.

[0004] Therefore, providing a low-temperature rate lithium-ion battery with low-temperature and high-rate charge and discharge performance has become an urgent problem to be solved. Summary of the invention

[0005] In order to solve the above problems existing in the prior art, the present invention provides a low-temperature rate lithium-ion battery and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0006] A first aspect of the present invention provides a low-temperature rate lithium-ion battery, comprising a plurality of positive electrode sheets and a plurality of negative electrode sheets opposite to the plurality of positive electrode sheets;

[0007] The positive electrode material on the surface of the positive electrode sheet includes Li 3x La 2 / 3-x The positive electrode active material formed by TiO3 coating on the surface of lithium iron phosphate, wherein the value of x ranges from 0.1 to 0.3;

[0008] The negative electrode material on the surface of the negative electrode sheet includes Sn z Li y , LiTi2(PO4)3 coated on the surface of hard carbon to form a negative electrode active material, wherein the value range of z is 1-22, and the value range of y is 1-5.

[0009] In a specific embodiment, the median particle size of the positive electrode active material is 2.0 to 5.0 μm, and the gram capacity is 140 to 145 mAh / g;

[0010] The Li 3x La 2 / 3-x The coating thickness of TiO3 is less than 5nm.

[0011] In a specific embodiment, the median particle size of the negative electrode active material is 2.0 to 4.0 μm, and the specific surface area is 3 to 5 m 2 / g, and the gram capacity is 320~330mAh / g.

[0012] In a specific embodiment, it also includes a plurality of diaphragms;

[0013] At least one separator is disposed between adjacent positive electrode sheets and negative electrode sheets.

[0014] In a specific embodiment, the plurality of positive electrode sheets, the plurality of negative electrode sheets and the plurality of separators form a laminated battery cell or a wound battery cell.

[0015] In a specific embodiment, the diaphragm includes a main material and an aromatic polyamide coated on at least one surface of the main material; the thickness of the aromatic polyamide is 4 to 6 um;

[0016] The main material includes one of a polyolefin film, a polyimide film, a spandex or aramid film, and a cellulose nanofiber film, and has a thickness of 16 to 20 um.

[0017] In a specific embodiment, it further includes an electrolyte; the plurality of positive electrode sheets and the plurality of negative electrode sheets are both located in the electrolyte;

[0018] The electrolyte includes the following components in percentage by mass:

[0019] LiPF6, 16-17 wt%;

[0020] Solvent, 73-84 wt%;

[0021] Additives, 3-5wt%.

[0022] In a specific embodiment, the solvent includes one of EC, EMC, and PC;

[0023] The additive includes one or more of LiBOB and LiBF4.

[0024] In a specific embodiment, the positive electrode material includes, by weight percentage: 91-92 wt % of the positive electrode active material, 4-4.5 wt % of a polyvinylidene fluoride binder, and 4-4.5 wt % of conductive carbon black;

[0025] In terms of mass percentage, the negative electrode material comprises: 93-94 wt % of the negative electrode active material, 5-7 wt % of a polyvinylidene fluoride binder and 2-3 wt % of conductive carbon black.

[0026] A second aspect of the present invention provides a method for preparing a low-temperature rate lithium-ion battery, comprising the following steps:

[0027] S1: Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, and the positive electrode active material is prepared into a positive electrode material;

[0028] S2: coating the positive electrode material on the surface of the positive electrode foil to form a positive electrode sheet;

[0029] S3: Sn z Li y , LiTi2(PO4)3 is coated on the surface of hard carbon to form a negative electrode active material, and the negative electrode active material is prepared into a negative electrode material;

[0030] S4: coating the negative electrode material on the surface of the negative electrode foil to form a negative electrode sheet;

[0031] S5: Processing the positive electrode sheet and the negative electrode sheet according to a lithium-ion battery preparation process to obtain a lithium-ion battery.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The lithium ion battery of the present invention uses Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, which enables the lithium-ion battery to form a fast ion conduction channel to improve the kinetic performance of the ions. z Li y At least one of LiTi2(PO4)3 is coated on the hard carbon surface to form a negative electrode active material, so that the lithium-ion battery has good conductivity, high specific capacity and low overpotential at a higher rate, thereby enabling the lithium-ion battery to have low-temperature and high-rate charge and discharge performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a charge and discharge comparison curve at 25° C. of a low-temperature rate lithium-ion battery provided in an embodiment of the present invention and a lithium-ion battery provided in a comparative example;

[0035] Figure 2 It is a discharge comparison curve at -20°C of a low-temperature rate lithium-ion battery provided by an embodiment of the present invention and a lithium-ion battery provided by a comparative example. DETAILED DESCRIPTION

[0036] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0037] Embodiment 1

[0038] This embodiment provides a low-temperature rate lithium-ion battery, including a plurality of positive electrode sheets and a plurality of negative electrode sheets opposite to the positive electrode sheets. The positive electrode material on the surface of the positive electrode sheet includes Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, wherein the value of x ranges from 0.1 to 0.3. The negative electrode material on the surface of the negative electrode sheet includes Sn z Li y , LiTi2(PO4)3 coated on the surface of hard carbon to form a negative electrode active material, wherein the value range of z is 1-22, and the value range of y is 1-5.

[0039] Specifically, Li 3x La 2 / 3-x TiO3 has excellent ionic conductivity, low resistivity, excellent chemical stability and thermal stability. 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, which can form a fast ion conduction channel in lithium-ion batteries, thereby improving the kinetic performance of ions. z Li y At least one of LiTi2(PO4)3 is coated on the hard carbon surface to form a negative electrode active material, which can make the lithium-ion battery have good conductivity, high specific capacity and low overpotential at a higher rate, so that the lithium-ion battery provided in this embodiment has low-temperature and high-rate charge and discharge performance.

[0040] Specifically, the median particle size of the positive electrode active material is 2.0 to 5.0 μm, and the gram capacity is 140 to 145 mAh / g. 3x La 2 / 3-x The coating thickness of TiO3 is less than 5nm. The median particle size of the negative electrode active material is 2.0-4.0μm, and the specific surface area is 3-5m 2 / g, and the gram capacity is 320~330mAh / g.

[0041] The lithium-ion battery provided in this embodiment also includes a plurality of diaphragms. At least one diaphragm is disposed between adjacent positive and negative electrodes. The diaphragm includes a main material and an aromatic polyamide coated on at least one surface of the main material. The main material includes one of a polyolefin film, a polyimide film, a spandex or aramid film, and a cellulose nanofiber film. The thickness of the main material is 16 to 20 um, and the thickness of the aromatic polyamide is 4 to 6 um. Preferably, the aromatic polyamide is coated on one surface of the main material. One diaphragm or multiple diaphragms may be disposed between adjacent positive and negative electrodes. Preferably, one diaphragm may be disposed between adjacent positive and negative electrodes.

[0042] The present embodiment provides a plurality of positive electrode sheets, a plurality of negative electrode sheets and a plurality of separators to form a laminated battery cell or a wound battery cell. Preferably, the plurality of positive electrode sheets, a plurality of negative electrode sheets and a plurality of separators form a laminated battery cell, and the outer shell of the battery cell is an aluminum-plastic film. The plurality of positive electrode sheets are welded to the positive electrode ears, and the positive electrode ears are aluminum-copper-plated nickel-plated ears, and the plurality of negative electrode sheets are welded to the negative electrode ears, and the negative electrode ears are copper-plated nickel-plated ears.

[0043] The lithium-ion battery provided in this embodiment also includes an electrolyte; a plurality of positive electrode sheets, a plurality of negative electrode sheets and a plurality of separators are all located in the electrolyte. The electrolyte includes the following components in mass percentage:

[0044] LiPF6, 16-17 wt%;

[0045] Solvent, 73-84 wt%;

[0046] Additives, 3-5wt%.

[0047] The solvent includes one of EC, EMC and PC, and the additive includes one or more of LiBOB and LiBF4.

[0048] Specifically, the concentration of LiPF6 in the electrolyte is 2.5 to 3.6 mol / L.

[0049] Specifically, the positive electrode material includes, by mass percentage, 91-92 wt% of positive electrode active material, 4-4.5 wt% of polyvinylidene fluoride binder, and 4-4.5 wt% of conductive carbon black. The negative electrode material includes, by mass percentage, 93-94 wt% of negative electrode active material, 5-7 wt% of polyvinylidene fluoride binder, and 2-3 wt% of conductive carbon black.

[0050] This embodiment provides a low-temperature rate lithium-ion battery, by using Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, which can form a fast ion conduction channel in lithium-ion batteries, thereby improving the kinetic performance of ions. z Liy At least one of LiTi2(PO4)3 is coated on the hard carbon surface to form a negative electrode active material, which can make the lithium-ion battery have good conductivity, high specific capacity and low overpotential at a higher rate, so that the lithium-ion battery provided in this embodiment has low-temperature and high-rate charge and discharge performance.

[0051] Embodiment 2

[0052] This embodiment provides a method for preparing a low-temperature rate lithium-ion battery, comprising the following steps:

[0053] S1: Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, and the positive electrode active material is prepared into a positive electrode material.

[0054] Specifically, Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material. 91-92wt% of the positive electrode active material, 4-4.5wt% of polyvinylidene fluoride binder, and 4-4.5wt% of conductive carbon black are added into a blender, and N-methylpyrrolidone NMP is added. The positive electrode material is prepared by wet stirring and a subsequent spiral dispersion process.

[0055] S2: coating the positive electrode material on the surface of the positive electrode foil to form a positive electrode sheet.

[0056] Specifically, the positive electrode material obtained in step S1 is coated on aluminum foil by a coating machine and baked by dry circulating air to obtain a positive electrode sheet.

[0057] S3: Sn z Li y At least one of LiTi2(PO4)3 is coated on the surface of hard carbon to form a negative electrode active material, and the negative electrode active material is prepared into a negative electrode material.

[0058] Specifically, coconut shells were carbonized, soaked in alkaline solution, purified and subjected to chemical vapor deposition (CVD) to prepare hard carbon. z Li y At least one of LiTi2(PO4)3 is coated on the surface of hard carbon to form a negative electrode active material, 93-94wt% of the negative electrode active material, 2-3wt% of the conductive carbon black, and 5-7wt% of the polyvinylidene fluoride binder are added to a blender, and NMP is added to obtain the negative electrode material by wet stirring and subsequent spiral dispersion process.

[0059] S4: coating the negative electrode material on the surface of the negative electrode foil to form a negative electrode sheet.

[0060] Specifically, the positive electrode material obtained in step S3 is coated on a copper foil by a coating machine and baked by dry circulating air to obtain a negative electrode sheet.

[0061] S5: Processing the positive electrode sheet and the negative electrode sheet according to the lithium ion battery preparation process to obtain a lithium ion battery.

[0062] Specifically, the positive electrode sheet obtained in step S2 and the negative electrode sheet obtained in step S4 are subjected to roller pressing, wherein the negative electrode sheet is subjected to hot pressing at a temperature of 135° C. The positive electrode sheet and the negative electrode sheet after roller pressing are prepared into a low-temperature rate lithium-ion battery according to the lithium-ion battery preparation process of die cutting-lamination-welding of pole tabs-assembly-baking-liquid injection-formation-capacity division-aging.

[0063] This embodiment provides a method for preparing a low-temperature rate lithium-ion battery, wherein Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material, and the positive electrode active material is prepared into a positive electrode material and coated on the surface of the positive electrode foil to form a positive electrode sheet, which can enable the lithium-ion battery to form a fast ion conduction channel, thereby improving the kinetic performance of the ions, and using Sn z Li y At least one of LiTi2(PO4)3 is coated on the surface of hard carbon to form a negative electrode active material, and the negative electrode active material is prepared into a negative electrode material and coated on the surface of the negative electrode foil to form a negative electrode sheet, which can make the lithium ion battery have good conductivity, high specific capacity and low overpotential at a higher rate, so that the lithium ion battery provided in this embodiment has low-temperature and high-rate charge and discharge performance.

[0064] Embodiment 3

[0065] This embodiment provides a low-temperature rate lithium-ion battery based on the first embodiment, including a plurality of positive electrode sheets and a plurality of negative electrode sheets opposite to the positive electrode sheets. The positive electrode material on the surface of the positive electrode sheet includes Li 3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form the positive electrode active material. The negative electrode material on the surface of the negative electrode sheet includes Sn z Li y and LiTi2(PO4)3 coated on the hard carbon surface to form the negative electrode active material. In this embodiment, x is 0.11, z is 5, y is 2, Sn z Li y The mass ratio of LiTi2(PO4)3 is 1:1.

[0066] The preparation method of the low-temperature rate lithium-ion battery provided in this embodiment includes:

[0067] S1: Li3x La 2 / 3-x TiO3 is coated on the surface of lithium iron phosphate to form a positive electrode active material. 92wt% of the positive electrode active material, 4wt% of the polyvinylidene fluoride binder, and 4wt% of the conductive carbon black are added into a mixer, and NMP is added to prepare the positive electrode material by wet stirring and subsequent spiral dispersion process.

[0068] S2: The positive electrode material obtained in step S1 is coated on aluminum foil by a coating machine, and baked by dry circulating air to obtain a positive electrode sheet.

[0069] S3: Sn z Li y and LiTi2(PO4)3 are coated on the hard carbon surface to form a negative electrode active material, 91.9wt% of the negative electrode active material, 2.8wt% of the conductive carbon black, and 5.3wt% of the polyvinylidene fluoride binder are added into a blender, NMP is added, and the negative electrode material is prepared by wet stirring and subsequent spiral dispersion process.

[0070] S4: coating the positive electrode material obtained in step S3 on copper foil by a coating machine, and baking with dry circulating air to obtain a negative electrode sheet.

[0071] S5: Roll-pressing the positive electrode sheet obtained in step S2 and the negative electrode sheet obtained in step S4, wherein the negative electrode sheet is hot-pressed at a temperature of 135° C. The rolled positive electrode sheet and the negative electrode sheet are prepared into a low-temperature rate lithium-ion battery according to the lithium-ion battery preparation process of die-cutting-lamination-welding of tabs-assembly-baking-liquid injection-formation-capacity division-aging.

[0072] Comparative Example 1

[0073] This comparative example provides a lithium ion battery, which is different from the third embodiment in that the positive electrode material on the surface of the positive electrode sheet includes lithium iron phosphate, and the negative electrode material on the surface of the negative electrode sheet includes hard carbon.

[0074] The preparation method of the lithium ion battery provided in this comparative example comprises:

[0075] Step 1: Add 92wt% of lithium iron phosphate, 4wt% of polyvinylidene fluoride binder, and 4wt% of conductive carbon black into a mixer, add NMP, and prepare positive electrode slurry by wet stirring and subsequent spiral dispersion process, coat it on aluminum foil through a coater, and bake it with dry circulating air to obtain positive electrode sheets.

[0076] Step 2: Add 91.5wt% of hard carbon, 2.5wt% of conductive carbon black, and 6wt% of polyvinylidene fluoride binder into a mixer, add NMP, and prepare the positive electrode slurry by wet stirring and subsequent spiral dispersion process. Coat it on copper foil through a coater and bake it with dry circulating air to obtain a negative electrode sheet.

[0077] Step 3: Roll the positive and negative electrodes, with the negative electrode being hot pressed at 135°C. Prepare the rate-type lithium-ion battery according to the process of die cutting - lamination - welding of tabs - assembly - baking - injection - formation - capacity division - aging.

[0078] The lithium ion batteries provided in Example 3 and Comparative Example 1 were tested. The charge and discharge comparison curves of the lithium ion batteries provided in Example 3 and Comparative Example 1 at 25° C. are as follows: Figure 1 As shown, the discharge comparison curves of the lithium ion batteries provided in Example 3 and Comparative Example 1 at -20°C are as follows: Figure 2 As shown, the test data of the lithium ion battery provided by Example 3 and Comparative Example 1 are shown in the following table:

[0079]

[0080] Depend on Figure 1 , Figure 2 As can be seen from the above table, the charging capacity, charging cross-current ratio, discharge capacity and discharge median voltage of the lithium ion battery provided in Example 3 are better than those of the lithium ion battery provided in Comparative Example 1, and it has good conductivity, high specific capacity and low overpotential at a higher rate, and still has good high-rate charge and discharge performance in low temperature environments of -20°C and -30°C.

[0081] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A low-temperature rate lithium-ion battery, It is characterized in that It includes a plurality of positive electrode sheets and a plurality of negative electrode sheets opposite to the plurality of positive electrode sheets; The positive electrode material on the surface of the positive electrode sheet includes Li 3x La 2 / 3-x TiO 3 A positive electrode active material coated on the surface of lithium iron phosphate, wherein the value of x ranges from 0.1 to 0.3; The negative electrode material on the surface of the negative electrode sheet includes Sn z Li y 、LiTi 2 (PO 4 ) 3 At least one of the negative electrode active materials is coated on the surface of hard carbon, wherein the value range of z is 1-22, and the value range of y is 1-5.

2. A low temperature rate lithium ion battery according to claim 1, It is characterized in that The median particle size of the positive electrode active material is 2.0 to 5.0 μm, and the gram capacity is 140 to 145 mAh / g; The Li 3x La 2 / 3-x TiO 3 The coating thickness is less than 5nm.

3. A low temperature rate lithium ion battery according to claim 1, It is characterized in that The median particle size of the negative electrode active material is 2.0 to 4.0 μm, and the specific surface area is 3 to 5 m 2 / g, and the gram capacity is 320~330mAh / g.

4. A low temperature rate lithium ion battery according to claim 1, It is characterized in that Also included are several diaphragms; At least one separator is disposed between adjacent positive electrode sheets and negative electrode sheets.

5. A low temperature rate lithium ion battery according to claim 4, It is characterized in that The plurality of positive electrode sheets, the plurality of negative electrode sheets and the plurality of separators form a laminated battery cell or a wound battery cell.

6. A low temperature rate lithium ion battery according to claim 4, It is characterized in that The diaphragm includes a main material and an aromatic polyamide coated on at least one surface of the main material; the thickness of the aromatic polyamide is 4 to 6 um; The main material includes one of a polyolefin film, a polyimide film, a spandex or aramid film, and a cellulose nanofiber film, and has a thickness of 16 to 20 um.

7. A low-temperature rate lithium-ion battery according to claim 1, It is characterized in that It also includes an electrolyte; the plurality of positive electrode sheets and the plurality of negative electrode sheets are all located in the electrolyte; The electrolyte includes the following components in percentage by mass: LiPF 6 ,16~17wt%; Solvent, 73-84 wt%; Additives, 3-5wt%.

8. A low-temperature rate lithium-ion battery according to claim 7, It is characterized in that The solvent includes one of EC, EMC and PC; The additives include LiBOB, LiBF 4 One or more of .

9. A low temperature rate lithium ion battery according to claim 1, It is characterized in that In terms of mass percentage, the positive electrode material comprises: 91-92 wt % of the positive electrode active material, 4-4.5 wt % of a polyvinylidene fluoride binder and 4-4.5 wt % of conductive carbon black; In terms of mass percentage, the negative electrode material comprises: 93-94 wt % of the negative electrode active material, 5-7 wt % of a polyvinylidene fluoride binder and 2-3 wt % of conductive carbon black.

10. A method for preparing a low-temperature rate lithium-ion battery, It is characterized in that The following steps are involved: S1: Li 3x La 2 / 3-x TiO 3 Coating the surface of lithium iron phosphate to form a positive electrode active substance, and preparing the positive electrode active substance into a positive electrode material; S2: coating the positive electrode material on the surface of the positive electrode foil to form a positive electrode sheet; S3: Sn z Li y 、LiTi 2 (PO 4 ) 3 At least one of the above is coated on the surface of hard carbon to form a negative electrode active material, and the negative electrode active material is prepared into a negative electrode material; S4: coating the negative electrode material on the surface of the negative electrode foil to form a negative electrode sheet; S5: Processing the positive electrode sheet and the negative electrode sheet according to a lithium-ion battery preparation process to obtain a lithium-ion battery.

Citation Information

Patent Citations

  • Hydrographical rechargeable lithium or sodium ion battery

    CN101154745A

  • Titanium phosphate lithium material used for cathode of lithium ion battery and preparation method thereof

    CN101807696A

  • Composite anode material and synthesis method and application thereof

    CN103094580A

  • Novel high-performance aqueous lithium / sodium ion battery and manufacturing method thereof

    CN109192978A

  • Negative electrode material, composite negative electrode material and preparation method thereof, secondary battery and terminal equipment

    CN115000403A