Composite halide solid electrolyte, preparation method thereof and battery

Through the general structural formula of the composite halide solid electrolyte and the mechanical ball milling method, the problems of low conductivity, complex synthesis and high cost of the halide solid electrolyte in the existing technology are solved, and high-efficiency, low-cost electrochemical performance is achieved, which is suitable for Applications of all-solid-state batteries.

CN118738534APending Publication Date: 2024-10-01NINGBO EASTERN INSTITUTE FOR ADVANCED STUDY
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411018358.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing halide solid-state electrolytes have low ionic conductivity, complex and energy-consuming synthesis processes, and contain expensive rare earth metal elements, resulting in high costs and difficulty in large-scale application.

Method used

The general structural formula of the composite halide solid-state electrolyte is (AaBb)m@MXc. The solid-phase reaction is carried out through mechanical ball milling in an anhydrous and oxygen-free inert atmosphere. The synthesis route is simplified, energy consumption is reduced, and the synthesis conditions are improved by optimizing the synthesis conditions. ionic conductivity.

Benefits of technology

It achieves high ionic conductivity, low-cost electrochemical performance, simplifies the synthesis process, reduces energy consumption and environmental pollution, and is suitable for commercial applications of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738534A_ABST
    Figure CN118738534A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and provides a composite halide solid electrolyte, a preparation method thereof and a battery, the structural general formula of the solid electrolyte is (AaBb) m (at) (MXc) n, A represents at least one of Li, Na, K, Cu and Ag in the structural general formula; b represents at least one of S < 2->, OH <->, NH2 <->, O2 < 2->, O2 <-> and N3 <-> in the structural general formula; m represents at least one of Zr, Hf, Ta, Nb, Al, Fe and Ga in the structural general formula; x represents at least one of F, Cl, Br and I in the structural general formula. The composite solid electrolyte provided by the invention is high in ionic conductivity, simple in synthetic technical route, low in raw material cost and good in electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of battery materials, and in particular relates to a composite halide solid electrolyte and a preparation method thereof, and a battery. Background Art

[0002] All-solid-state batteries have become the most promising next-generation energy storage technology due to their high energy density and high safety. The development of solid electrolytes with high ionic conductivity, wide electrochemical stability window and controllable cost is the key to the practical application of all-solid-state batteries. Halide solid electrolytes have received great attention from academia and industry due to their high oxidation stability and the fact that they do not react with air to release toxic gases.

[0003] Existing relevant technical literature shows that halide solid electrolytes conduct Li + Ion (or Na + , K + 、Ag + etc., with Li + ions as an example) are mainly three ways: 1. With halogen anions (Cl - Br - ,I - ) are densely packed to form a crystalline phase halide solid electrolyte for transport channels, Li + Ions are transported along the "octahedron-tetrahedron-octahedron" channel or "octahedron-octahedron" channel, such as Li3InCl6; 2. Crystalline halide solid electrolytes with UCl3-type lattice transport channels, Li + Ions are mainly conducted in one-dimensional channels surrounded by three-capped triangular prisms with common edges, such as Li 0.388 Ta 0.238 La 0.475 Cl3; 3. Composite solid electrolyte composed of oxide and halide, Li + Ions are mainly transported at the interface between halide grains and oxide grains, such as LiBH4-LiI / Al2O3.

[0004] However, the halide solid electrolytes disclosed in the relevant technical literature still have some bottleneck problems:

[0005] 1. Ionic conductivity (for example: Li3InCl6 is about 1.36×10 -3 S cm -1 ) is still not high enough.

[0006] 2. The technical route for synthesizing crystalline halide solid electrolytes involves rigorous steps such as high temperature and sintering under vacuum, which has high energy consumption and is difficult to apply on a large scale.

[0007] III. The inclusion of expensive rare earth metal elements (including Sc, Y, and La series elements) results in high raw material costs. Summary of the Invention

[0008] The purpose of this application is to provide a composite halide solid electrolyte, its preparation method, and a battery, aiming to improve the conductivity, reduce the raw material cost, and simplify the synthesis route.

[0009] To achieve the above application purpose, the technical solutions adopted in this application are as follows:

[0010] In the first aspect, this application provides a composite halide solid electrolyte, and the structural general formula of the composite halide solid electrolyte is: (A a B b ) m @MX c Wherein: A represents at least one of Li, Na, K, Cu, and Ag in the structural general formula; B represents at least one of S 2- , OH - , NH 2- , O2 2- , O 2- , and N 3- ; M represents at least one of Zr, Hf, Ta, Nb, Al, Fe, and Ga in the structural general formula; X represents at least one of F, Cl, Br, and I in the structural general formula; a and b respectively represent the corresponding atomic numbers in the A a B b compound, a is 1 or 2 or 3, and b is 1. c represents the corresponding atomic number in the MX c compound, c is 3 or 4 or 5; m represents the amount of substance of the A a B b compound, 0 < m < 5. The composite solid electrolyte provided in this application has high ionic conductivity, a simple synthesis technical route, low raw material costs, and good electrochemical performance.

[0011] In the second aspect, this application provides a preparation method of a composite halide solid electrolyte, including the following steps: under an anhydrous and oxygen-free inert atmosphere, subject the raw materials A a B b and MX c to a solid-phase reaction by mechanical ball milling to obtain the composite halide solid electrolyte (A a B b ) m @MX c . The preparation method provided in the embodiments of this application has a simple process, a short cycle, does not involve high-temperature and vacuum sintering operations, does not generate irritating gases, and can significantly reduce energy consumption and environmental pollution.

[0012] In a third aspect, the present application provides a battery comprising the composite halide solid electrolyte described above, or the composite halide solid electrolyte obtained by the preparation method described above. The battery is an all-solid-state battery. The types of batteries include lithium-ion batteries, sodium-ion batteries, potassium-ion batteries, silver-ion batteries or copper-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0014] Figure 1 Electrochemical AC impedance spectra of the halide solid electrolytes Li2O@ZrCl4, Li2S@ZrCl4, Li3N@ZrCl4 provided in Example 1 of the present application and the halide solid electrolyte Li2ZrCl6 provided in Comparative Example 1.

[0015] In the figure, the horizontal axis represents the real resistance, the unit is ohm (Ω); the vertical axis represents the imaginary resistance, the unit is ohm (Ω), and the spectrum lines a, b, c and d represent Li2O@ZrCl4, Li2S@ZrCl4, Li3N@ZrCl4 and Li2ZrCl6 respectively.

[0016] Figure 2 X-ray diffraction spectra of the halide solid electrolytes Li2O@ZrCl4, Li2S@ZrCl4, Li3N@ZrCl4 provided in Example 1 of the present application and the halide solid electrolyte Li2ZrCl6 provided in Comparative Example 1.

[0017] In the figure, the horizontal axis represents the diffraction angle (2Theta), the unit is degree (°); the vertical axis represents the diffraction intensity; the diffraction lines a, b, c and d represent Li2O@ZrCl4, Li2S@ZrCl4, Li3N@ZrCl4 and Li2ZrCl6 respectively.

[0018] Figure 3 This is a high-resolution cryo-transmission electron microscopy photograph of the halide solid electrolyte Li2O@ZrCl4 provided in Example 1 of the present application.

[0019] In the figure, the illustration in the upper left corner is the diffraction spot.

[0020] Figure 4 This is the electrochemical impedance spectroscopy of the halide solid electrolyte Na2S@ZrCl4 provided in Example 2 of the present application.

[0021] In the figure, the horizontal axis represents the real resistance, and the unit is ohm (Ω); the vertical axis represents the imaginary resistance, and the unit is ohm (Ω).

[0022] Figure 5 This is the electrochemical impedance spectroscopy of the halide solid electrolyte Ag2O@ZrCl4 provided in Example 3 of the present application.

[0023] In the figure, the horizontal axis represents the real resistance, and the unit is ohm (Ω); the vertical axis represents the imaginary resistance, and the unit is ohm (Ω).

[0024] Figure 6 This is the charge and discharge curve of the all-solid-state lithium battery assembled in Example 4 of the present application.

[0025] In the figure, the horizontal axis represents the specific capacity, the unit is milliampere hour / gram (mAh g -1 ); the ordinate represents voltage (relative to Li + / Li voltage), the unit is volt (V); the solid line is the charge and discharge curve of the first week, and the dotted line is the charge and discharge curve of the second week.

[0026] Figure 7 The electrochemical performance of the all-solid-state lithium battery assembled in Example 4 of the present application at a 1C rate.

[0027] In the figure, the horizontal axis represents the number of cycles; the vertical axis on the left represents the specific capacity, the unit is milliampere hour / gram (mAh g -1 ); the vertical axis on the right represents the Coulomb efficiency.

[0028] Figure 8 This is the charge and discharge curve of the all-solid-state lithium battery assembled in Example 5 of the present application.

[0029] In the figure, the horizontal axis represents the specific capacity, the unit is milliampere hour / gram (mAh g -1 ); the ordinate represents voltage (relative to Li + / Li voltage), the unit is volt (V); the solid line is the charge and discharge curve of the first week, and the dotted line is the charge and discharge curve of the second week.

[0030] Fig. 9 This is the charge and discharge curve of the second week of the all-solid-state sodium battery assembled in Example 6 of the present application.

[0031] In the figure, the horizontal axis represents the specific capacity, the unit is milliampere hour / gram (mAh g -1 ); the ordinate represents voltage (relative to Na + / Na voltage), the unit is volt (V).

[0032] Fig.10 The electrochemical performance of the all-solid-state lithium battery assembled in Example 7 of the present application at -30°C.

[0033] In the figure, the horizontal axis represents the number of cycles; the vertical axis on the left represents the specific capacity, the unit is milliampere hour / gram (mAh g -1 ); the vertical axis on the right represents the Coulomb efficiency.

[0034] Fig.11 X-ray diffraction spectra of Li2S@ZrCl4, Li2S@TaCl5, and Na2S@ZrCl4 sulfur-halide compound solid electrolytes prepared in Examples 4 to 6 of the present application. In the figure, the horizontal axis represents the diffraction angle (2Theta), in degrees (°); the vertical axis represents the diffraction intensity.

[0035] Fig.12 X-ray diffraction spectra of Li2S@ZrCl4 sulfur halide solid electrolyte prepared with different ball milling times in Example 4 of the present application. In the figure, the horizontal axis represents the diffraction angle (2Theta), the unit is degree (°); the vertical axis represents the diffraction intensity.

[0036] Fig.13 This is the EDS surface scan of the Na2S-ZrCl4 sulfur-halide compound solid electrolyte synthesized in Example 6 of the present application, including the surface scans of Na, S, Zr, and Cl elements.

[0037] Fig.14 The charge and discharge curve of the all-solid-state lithium battery assembled in Example 14 of the present application at a rate of 0.1C for the first three weeks. In the figure, the horizontal axis represents the specific capacity in milliampere hours per gram (mAh g -1 ); the vertical axis represents voltage (voltage relative to Li+ / Li), and the unit is volt (V). DETAILED DESCRIPTION

[0038] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0039] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0040] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0041] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0042] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0043] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0044] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0045] In a first aspect, the present application provides a composite halide solid electrolyte, the general structural formula of which is: (A a B b ) m @MX c ,in:

[0046] A represents that the general structural formula contains at least one of Li, Na, K, Cu and Ag;

[0047] B indicates that the general structural formula contains S 2- OH - NH 2- 、O2 2- , O 2- and N 3- At least one of

[0048] M represents that the general structural formula contains at least one of Zr, Hf, Ta, Nb, Al, Fe and Ga;

[0049] X represents that the general structural formula contains at least one of F, Cl, Br and I;

[0050] a and b represent A a B b The corresponding number of atoms in the compound, a is 1, 2, or 3, and b is 1. c represents MX c The corresponding number of atoms in the compound, c is 3, 4 or 5; m represents A a B b The amount of substance of the compound, 0 <m<5。

[0051] The composite solid electrolyte provided in the embodiments of the present application has high ionic conductivity, a simple synthesis technology route, low raw material cost, and good electrochemical performance.

[0052] The composite halide solid electrolyte provided in the embodiment of the present application is composed of the main raw material A a B b and MX c Made in MX c Made into a dispersed matrix, solid A a B b Will be evenly dispersed in the matrix MX c In the solid phase dispersion system, MX c It can be combined with various metal salts (LiCl, Li2O, Li3N, Na2S, etc.) to synthesize solid electrolytes and has strong universality.

[0053] In some embodiments, the general structural formula of the composite halide solid electrolyte is: a B b ) m @MX c , where: M indicates that the general structural formula contains Zr, and c is 4.

[0054] In the embodiment of the present application, the general structural formula of the composite halide solid electrolyte can be expressed as (A a B b ) m@ZrX4 is a zirconium-containing halide solid electrolyte with a structure in which a crystalline phase is embedded in an amorphous phase matrix. The way it conducts A ions is different from other existing halide solid electrolytes: it mainly conducts through the amorphous phase and can conduct Li + 、Na + , K + 、Ag + , Cu + By optimizing the synthesis conditions and increasing the relative content of the amorphous phase, Li + Ionic conductivity up to 3.0×10 -3 S cm -1 (Room temperature). The ZrX4 of the present invention can be combined with various metal salts (LiCl, Li2O, Li3N, Na2S, etc.) to synthesize solid electrolytes, which has strong universality. a B b ) m @ZrX4 halide solid electrolyte excellent Li + Ion conduction capability, the all-solid-state lithium battery assembled using halide solid electrolyte Li2O@ZrCl4 can serve in extreme working conditions of low temperature (-30℃).

[0055] In some embodiments, the general structural formula of the composite halide solid electrolyte is: a B b ) m @MX c , where: B means that the general structure contains S 2- , a is 2, b is 1.

[0056] The general structural formula of the composite halide solid electrolyte provided in the embodiment of the present application can be expressed as (A2S): m @MX c , is a sulfur-halide compound solid electrolyte. The sulfur-halide compound solid electrolyte contains a large amount of amorphous components, and the amorphous structure has a large free volume. The A ion jumping transmission in it is less repelled by the framework cations, so the ion conductivity is high. This material is synthesized using halide metal and A2S as raw materials. Compared with sulfide electrolytes, the electrolyte oxidation limit is significantly improved, which improves the capacity of the positive electrode active material and the energy density of the entire battery, and increases the possibility of solid-state battery application, thereby realizing the commercial application value of all-solid-state secondary batteries.

[0057] In some embodiments, additive A is also included x Z; Z means containing O2 2- , O 2- 、CO3 2- PO4 3- 、P2O7 4- 、SO42- At least one of the following; x is 2 or 3 or 4

[0058] In some embodiments, auxiliary additives may be added to the composite halide solid electrolyte, such as at least one of alkali metal elements, alkaline earth metal elements, transition metal elements and rare earth elements. The content of the auxiliary additives is 0 ≤ w % ≤ 20% relative to the overall mass of the composite halide solid electrolyte.

[0059] In some embodiments, the composite halide solid electrolyte comprises an amorphous phase and a crystalline phase, wherein grains of the crystalline phase are embedded in a matrix of the amorphous phase; the chemical composition of the crystalline phase comprises AX, and constituent ions of the amorphous phase comprise A, B, M, and X.

[0060] The carrier A ions are mainly conducted in the amorphous / crystalline phase matrix or between phases, and the room temperature ionic conductivity is relatively high, greater than 1*10 -5 S cm -1 .

[0061] In some embodiments, the raw material includes A a B b and MX c Among them, A a B b and MX c The amount of substance ratio is 0.2:1~351.

[0062] In some embodiments, raw material A a B b Including at least one of lithium hydroxide, sodium hydroxide, lithium amide, sodium amide, lithium peroxide, sodium peroxide, lithium oxide, sodium oxide, silver oxide, cuprous oxide, lithium sulfide, sodium sulfide, silver sulfide, cuprous sulfide and lithium nitride; and / or, the raw material MX c The invention comprises at least one of anhydrous zirconium tetrafluoride, anhydrous zirconium tetrachloride, anhydrous zirconium tetrabromide, anhydrous zirconium tetraiodide, anhydrous tantalum pentachloride and anhydrous silicon chloride.

[0063] A second aspect of the embodiment of the present application provides a method for preparing a composite halide solid electrolyte, comprising the following steps:

[0064] In an inert atmosphere without water or oxygen, raw material A a B b and MX c The composite halide solid electrolyte (A) was obtained by mechanical ball milling to produce a solid phase reaction. a B b ) m @MX c .

[0065] The preparation method provided in the embodiment of the present application has a simple process and a short cycle, does not involve high-temperature and vacuum sintering operations, does not produce irritating gases, and can significantly reduce energy consumption and environmental pollution.

[0066] The above-mentioned anhydrous and oxygen-free inert atmosphere is N2 or Ar gas. Further, Ar gas is used.

[0067] During the mechanical ball milling process, the ball mill tank needs to be effectively cooled to prevent the tank temperature from being too high. Furthermore, a circulating water cooling method is used.

[0068] In some embodiments, the mechanical ball milling control parameters include:

[0069] The grinding beads are one or more of grinding beads with a diameter of 3 mm to 10 mm;

[0070] and / or the total mass ratio of grinding beads to raw materials is 60:1 to 20:1;

[0071] And / or the ball milling time is 1h to 80h; the ball mill speed is 400r / min to 800r / min.

[0072] Furthermore, the grinding beads are one or more of grinding beads with a diameter of 3 mm to 10 mm; for example, the grinding beads have a diameter of 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm.

[0073] Furthermore, the total mass ratio of the grinding beads to the raw materials (i.e., the ball-to-material ratio) is 60:1 to 20:1; such as the material-to-ball ratio is 20:1, 30:1, 40:1, 50:1 or 60:1.

[0074] Furthermore, 3 mm grinding beads were used with a ball to material ratio of 30:1.

[0075] Further, the ball milling time is 1 h to 80 h, such as 1 h, 1.5 h, 2 h, 2.5 h, 3.5 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 20 h, 30 h, 40 h, 50 h, 60 h, 70 h, 80 h;

[0076] Furthermore, the rotation speed of the ball mill is 400 r / min to 800 r / min, such as 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min, and 800 r / min.

[0077] Furthermore, the ball milling time is 10 h, and the ball mill speed is 400 r / min.

[0078] In the composite halide solid electrolyte provided in the embodiment of the present application, the relative proportion of the amorphous phase and the crystalline phase is regulated by the synthesis conditions, including ball milling parameters (ball milling time, rotation speed), raw material ratio, etc. The optimization of each parameter improves the conductivity of the halide solid electrolyte to a certain extent; the higher the relative content of the amorphous phase, the higher the A ion conductivity.

[0079] In some embodiments, a premixing step is further included: raw material A is mixed under an inert atmosphere without water or oxygen. a B b and MX c The powders are pre-mixed to obtain pre-mixed powders; and the pre-mixed powders are processed by mechanical ball milling.

[0080] The above-mentioned anhydrous and oxygen-free inert atmosphere is N2 or Ar gas, and preferably, Ar gas is used.

[0081] The premixing can be carried out by hand grinding in a mortar, mixing in a mixer, or the like.

[0082] Furthermore, the preparation method of the halide solid electrolyte specifically includes:

[0083] First, in an inert atmosphere without water or oxygen, the raw material powder A a B b and MX c Premix in a certain proportion.

[0084] Then, in an inert atmosphere without water or oxygen, the pre-mixed powder in the previous step is transferred to a ball mill, and an appropriate amount of grinding beads is added and sealed; the raw material powder A is made into a B b and MX c Solid phase reaction occurs to obtain a halide solid electrolyte (A a B b ) m @MX c .

[0085] Before the ball mill is sealed, the ball mill can be evacuated or kept in an inert atmosphere; preferably, a vacuum operation is performed.

[0086] A third aspect of an embodiment of the present application provides a battery, comprising the above-mentioned composite halide solid electrolyte, or the composite halide solid electrolyte obtained by the above-mentioned preparation method.

[0087] In some embodiments, the battery is an all-solid-state battery.

[0088] In some embodiments, the type of battery includes a lithium ion battery, a sodium ion battery, a potassium ion battery, a silver ion battery, or a copper ion battery.

[0089] In some embodiments, an all-solid-state lithium battery includes a positive electrode sheet, a negative electrode sheet, and a solid electrolyte sheet between the positive and negative electrodes.

[0090] The solid electrolyte sheet is obtained by cold pressing a solid electrolyte material, and the solid electrolyte material is the above-mentioned composite halide solid electrolyte or a solid electrolyte prepared by the above-mentioned composite halide solid electrolyte preparation method.

[0091] The positive electrode sheet is obtained by cold pressing or coating the positive electrode active material and the positive electrode filler. The positive electrode active material includes but is not limited to at least one of cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxide, and lithiated layered sulfide. The positive electrode filler is at least one of an ion conductor, a conductive agent, and an adhesive; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are of the same material; the conductive agent may include at least one of graphite, carbon black, acetylene black, Ketjen black, and carbon fiber; the adhesive may include, for example, at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Cold pressing or coating methods are common methods for preparing positive electrode sheets in the art.

[0092] The negative electrode sheet is obtained by cold pressing or coating the negative electrode active material and the negative electrode filler. The negative electrode active material refers to the material that can store and release Li + Ionic materials include but are not limited to metal materials, graphite, and silicon; metal materials can be single metals or alloys; when metal materials are used as negative electrode active materials, negative electrode fillers can be omitted. Negative electrode fillers are at least one of ion conductors, conductive agents, and adhesives; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are of the same material; the conductive agent may include at least one of graphite, carbon black, acetylene black, Ketjen black, and carbon fiber; the adhesive may include, for example, at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Cold pressing or coating methods are common methods for preparing negative electrode sheets in this field.

[0093] In some embodiments, an all-solid-state sodium battery includes a positive electrode, a negative electrode, and a solid electrolyte between the positive and negative electrodes.

[0094] The solid electrolyte is the above-mentioned composite halide solid electrolyte or a solid electrolyte prepared by the preparation method of the above-mentioned composite halide solid electrolyte.

[0095] The positive electrode includes a positive electrode active material and a positive electrode filler. The positive electrode active material includes but is not limited to at least one of sodium-containing layered oxides, polyanionic compounds and Prussian blue compounds. The positive electrode filler is at least one of an ion conductor, a conductive agent and an adhesive; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are of the same material; the conductive agent may include at least one of graphite, carbon black, acetylene black, Ketjen black and carbon fiber; the adhesive may include at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride and polyethylene.

[0096] The negative electrode includes negative electrode active materials and negative electrode fillers. Negative electrode active materials refer to materials that can store and release Na + Ionic materials include but are not limited to metal materials and hard carbon; the metal material can be a single metal or an alloy. The negative electrode filler is at least one of an ion conductor, a conductive agent and an adhesive; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are of the same material; the conductive agent may include at least one of graphite, carbon black, acetylene black, Ketjen black and carbon fiber; the adhesive may include at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride and polyethylene. The all-solid-state sodium battery can be assembled according to conventional methods in the art.

[0097] The following describes the invention in conjunction with specific embodiments.

[0098] Example 1

[0099] This embodiment provides composite halide solid electrolytes Li2O@ZrCl4, Li2S@ZrCl4 and Li3N@ZrCl4, and the specific preparation method is as follows:

[0100] In an argon atmosphere glove box without water or oxygen, Li2O and ZrCl4 were mixed in a molar ratio of 1:1 and hand-ground with an agate mortar for 10 min to mix them thoroughly.

[0101] The mixed powder (about 2g) was transferred to a 75mL ball mill, and 60g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 550 rpm for 20h. The ball mill was cooled with circulating water during the ball milling process. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2O@ZrCl4 halide solid electrolyte.

[0102] According to the above steps, Li2S@ZrCl4 and Li3N@ZrCl4 halide solid electrolytes were synthesized respectively. The difference is that the raw material Li2O is replaced by Li2S and Li3N respectively.

[0103] Example 2

[0104] This embodiment provides a composite halide solid electrolyte Na2S@ZrCl4.

[0105] The Na2S@ZrCl4 halide solid electrolyte was synthesized specifically according to the preparation method provided in Example 1, except that the raw material Li2O was replaced by Na2S.

[0106] Example 3

[0107] This embodiment provides a composite halide solid electrolyte Ag2O@ZrCl4.

[0108] Specifically, the Ag2O@ZrCl4 halide solid electrolyte was synthesized according to the preparation method provided in Example 1, except that the raw material Li2O was replaced by Ag2O.

[0109] Example 4

[0110] This embodiment provides a composite halogen compound solid electrolyte Li2S@ZrCl4, and the specific preparation method is as follows:

[0111] In an argon atmosphere glove box without water or oxygen, Li2S and ZrCl4 were mixed in a substance ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0112] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600r / min for 5h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2S@ZrCl4 composite halogen compound solid electrolyte.

[0113] Example 5

[0114] This embodiment provides a composite halogen compound solid electrolyte Li2S@TaCl5.

[0115] Specifically, the Li2S@TaCl5 composite halogen compound solid electrolyte was synthesized according to the preparation method provided in Example 4, except that the raw material ZrCl4 was replaced by TaCl5, and the ball milling time was replaced from 5 h to 3 h.

[0116] Example 6

[0117] This embodiment provides a composite halogen compound solid electrolyte Na2S@ZrCl4.

[0118] Specifically, the Na2S@ZrCl4 composite halogen compound solid electrolyte was synthesized according to the preparation method provided in Example 4, except that the raw material Li2S was replaced by Na2S.

[0119] Example 7

[0120] This embodiment provides a composite halogen compound solid electrolyte Ag2S@TaCl5.

[0121] Specifically, the Ag2S@TaCl5 composite halogen compound solid electrolyte was synthesized according to the preparation method provided in Example 4, except that the raw material ZrCl4 was replaced by TaCl5, the raw material Li2S was replaced by Ag2S, and the ball milling time was replaced from 5h to 3h.

[0122] Example 8

[0123] This embodiment provides a composite halogen compound solid electrolyte Na2S@TaCl5.

[0124] Specifically, the Na2S@TaCl5 composite halogen compound solid electrolyte was synthesized according to the preparation method provided in Example 4, except that the raw material ZrCl4 was replaced by TaCl5, the raw material Li2S was replaced by Na2S, and the ball milling time was replaced from 5 h to 3 h.

[0125] Example 9

[0126] This embodiment provides a sulfur-halide compound solid electrolyte Li2S@ZrCl4+0.2SiCl4, wherein 0.2SiCl4 is an auxiliary additive.

[0127] Specifically, Li2S@ZrCl4+0.2SiCl4-sulfur halide solid electrolyte was synthesized according to the preparation method provided in Example 4, except that the raw materials and their amounts were replaced with Li2S, SiCl4 and ZrCl4 mixed in a molar ratio of 1:0.2:1.

[0128] Example 10

[0129] This embodiment provides an all-solid-state lithium battery, which is assembled using the halide solid electrolyte Li2O@ZrCl4 provided in Example 1. The specific assembly process is as follows:

[0130] Step 1: Weigh 120 mg of the halide solid electrolyte Li2O@ZrCl4 powder synthesized in Example 1, and cold press it into a solid electrolyte sheet with a diameter of 10 mm at a pressure of 100 MPa for 2 minutes.

[0131] Step 2: Weigh the commercially available lithiated layered oxide LiNi 0.88 Co 0.06 Mn 0.06 O2 (as positive electrode active material) and Li2O@ZrCl4 (as ion conductor) with a mass ratio of 7:3 were manually ground in a mortar for 10 min until uniformly mixed; 10 mg of the mixed powder was weighed and evenly spread on one side of the solid electrolyte sheet prepared in step 1, and cold pressed at a pressure of 350 MPa for 2 min to form a double-layer structure of "positive electrode sheet-solid electrolyte sheet".

[0132] Step 3: Use a commercially available indium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material, and stick it on the other surface of the solid electrolyte sheet in the double-layer structure prepared in step 2 to form a three-layer structure of "positive electrode sheet-solid electrolyte sheet-negative electrode sheet". Apply a pressure of 75 MPa to the whole structure, and complete the assembly to obtain an all-solid-state lithium battery.

[0133] The steps 1 to 3 are all carried out in a glove box with an anhydrous and oxygen-free argon atmosphere.

[0134] Embodiment 11

[0135] This embodiment provides an all-solid-state lithium battery, which is assembled using the halide solid electrolyte Li2O@ZrCl4 provided in Example 1. The specific assembly process is as shown in Example 10, except that the indium sheet used in step 3 is replaced by a lithium sheet (with a diameter of 10 mm and a thickness of 100 μm) as the negative electrode active material.

[0136] Example 12

[0137] This embodiment provides an all-solid-state sodium battery, which is assembled using the halide solid electrolyte Na2S@ZrCl4 provided in Example 2. The specific assembly process is as shown in Example 10, except that:

[0138] The Li2O@ZrCl4 halide solid electrolyte used in step 1 is replaced with Na2S@ZrCl4 halide solid electrolyte;

[0139] The positive electrode active material LiNi used in step 2 0.88 Co 0.06 Mn 0.06 O2 and ion conductive agent Li2O@ZrCl4 were replaced by Na2MnO3 and Na2S@ZrCl4, respectively.

[0140] The indium sheet used in step 3 was replaced with a sodium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material.

[0141] Embodiment 13

[0142] This embodiment provides an all-solid-state lithium battery, which is assembled using the halide solid electrolyte Li2O@ZrCl4 provided in Example 1. The specific assembly process is as shown in Example 10, except that the indium sheet used in step 3 is replaced by a lithium-indium alloy sheet (with a diameter of 10 mm and a thickness of 300 μm) as the negative electrode active material.

[0143] Embodiment 14

[0144] This embodiment provides an all-solid-state lithium battery, which is assembled using the sulfur-halogen compound solid electrolyte Li2S@ZrCl4 provided in Example 1. The specific assembly process is as follows:

[0145] Step 1: Weigh the commercially available lithiated layered oxide LiNi 0.88 Co 0.06 Mn 0.06O2 (as positive electrode active material), Li2S@ZrCl4 (as ion conductor) and carbon black (as electronic conductor) with a mass ratio of 7:3:0.1 were manually ground in a mortar for 10 min until uniformly mixed to form a composite positive electrode.

[0146] Step 2: Weigh 50 mg of the sulfur-halogen compound solid electrolyte Li2S@ZrCl4 powder synthesized in Example 1, cold press it into a solid electrolyte sheet with a diameter of 10 mm, and keep the pressure at 100 MPa for 2 min. Weigh 50 mg of Li6PS5Cl as a barrier layer between the sulfur-halogen compound solid electrolyte Li2S@ZrCl4 and the LiIn negative electrode, evenly spread it on one side of the Li2S@ZrCl4 solid electrolyte sheet, cold press it at a pressure of 100 MPa, and keep the pressure for 2 min.

[0147] Step 3: Weigh 10 mg of the composite positive electrode prepared in step 1, evenly spread it on the other side of the Li2S@ZrCl4 solid electrolyte sheet prepared in step 2, and cold press it at a pressure of 350 MPa for 2 minutes.

[0148] Step 4: Use a commercially available indium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material and stick it on the other side of the Li6PS5Cl barrier layer prepared in step 2 to form a three-layer structure of "positive electrode sheet-solid electrolyte sheet-barrier layer-negative electrode sheet". Apply a pressure of 100 MPa to the whole structure, and complete the assembly to obtain an all-solid-state lithium battery.

[0149] The steps 1 to 4 are all carried out in a glove box with an anhydrous and oxygen-free argon atmosphere.

[0150] Comparative Example 1

[0151] This case provides a solid electrolyte, and the specific preparation method is as follows:

[0152] In an anhydrous and oxygen-free argon atmosphere glove box, LiCl and ZrCl4 were mixed at a molar ratio of 2:1 and hand-ground using an agate mortar for 10 min to fully mix.

[0153] The mixed powder (about 2g) was transferred to a 75mL ball mill, and 60g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 550 rpm for 20h. The ball mill was cooled with circulating water during the ball milling process. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2ZrCl6 halide solid electrolyte.

[0154] 1. Characterization and Analysis

[0155] 1. Characterization and analysis of ionic conductivity

[0156] (1) Characterization methods

[0157] In a glove box with an argon atmosphere without water or oxygen, the solid electrolyte powders prepared in Examples 1-8 and Comparative Example 1 were filled into a cylindrical tablet pressing mold (with a diameter of 10 mm); and cold pressed at a pressure of 375 MPa for 2 min to obtain a solid electrolyte sheet with a thickness of 0.5 mm to 1.5 mm and a diameter of 10 mm; after gold plating on the upper and lower surfaces of the solid electrolyte sheet, two stainless steel blocking electrodes were used to clamp the upper and lower surfaces, and the electrochemical workstation was connected to test the electrochemical AC impedance spectrum at room temperature; room temperature Li + Ionic conductivity.

[0158] (2) Characterization results

[0159] The electrochemical impedance spectroscopy of the halide solid electrolytes Li2O@ZrCl4, Li2S@ZrCl4, Li3N@ZrCl4 synthesized in Example 1 and the halide solid electrolyte Li2ZrCl6 synthesized in Comparative Example 1 is shown in Figure 1 shown.

[0160] The electrochemical impedance spectroscopy of the halide solid electrolyte Na2S@ZrCl4 synthesized in Example 2 is as follows: Figure 4 shown.

[0161] The electrochemical impedance spectroscopy of the halide solid electrolyte Ag2O@ZrCl4 synthesized in Example 3 is shown in Figure 5 shown.

[0162] From the electrochemical impedance spectroscopy characterized above, the corresponding ionic conductivity was obtained, as shown in Table 1.

[0163] Table 1 Ionic conductivity test results of solid electrolytes

[0164] sample <![CDATA[Ionic conductivity S cm -1 > <![CDATA[Li2ZrCl6 (Comparative Example 1)]]> <![CDATA[0.3×10 -3 ]]> <![CDATA[Li2O@ZrCl4 (Example 1)]]> <![CDATA[3.0×10 -3 ]]> <![CDATA[Li2S@ZrCl4 (Example 1)]]> <![CDATA[1.2×10 -3 ]]> <![CDATA[Li3N@ZrCl4 (Example 1)]]> <![CDATA[0.6×10 -3 ]]> <![CDATA[Na2S@ZrCl4 (Example 2)]]> <![CDATA[0.5×10 -3 ]]> <![CDATA[Ag2O@ZrCl4 (Example 3)]]> <![CDATA[2.9×10 -3 ]]> <![CDATA[Li2S@ZrCl4 (Example 4)]]> <![CDATA[1.74×10 -3 ]]> <![CDATA[Na2S@ZrCl4 (Example 5)]]> <![CDATA[0.23×10 -3 ]]> <![CDATA[Li2S@TaCl5 (Example 6)]]> <![CDATA[2.45×10 -3 ]]> <![CDATA[Na2S@TaCl5 (Example 7)]]> <![CDATA[1.03×10 -3 ]]> <![CDATA[Ag2S@TaCl5 (Example 8)]]> <![CDATA[4.95×10 -3 ]]>

[0165] 2. Crystal structure characterization and analysis

[0166] (1) Characterization methods

[0167] The solid electrolytes prepared in Example 1, Examples 4-6 and Comparative Example 1 were characterized using an X-ray diffractometer.

[0168] (2) Characterization results

[0169] like Figure 2 As shown, the crystal structures of the halide solid electrolytes Li2O@ZrCl4, Li2S@ZrCl4, and Li3N@ZrCl4 synthesized in Example 1 are respectively characterized.

[0170] The results show that the three halide solid electrolytes provided in Example 1 all exhibit broadened diffraction peaks, which can be labeled as LiCl (space group Fm-3m), indicating that most of the three halide solid electrolytes are disordered amorphous phases, containing a small amount of crystalline phase, which is LiCl. The Li2ZrCl6 halide solid electrolyte provided in Comparative Example 1 has an obvious diffraction peak, which can be labeled as Li2ZrCl6 (space group P-3m1), indicating that the halide solid electrolyte is a crystalline phase Li2ZrCl6, and has a low degree of crystallinity.

[0171] like Fig.11 It is shown that the three composite halogen compound solid electrolytes provided in the embodiment all exhibit broadened diffraction peaks, which can be calibrated as residual raw materials Li2S or ACl (LiCl or NaCl, space group is Fm-3m), indicating that most of the above three sulfur-halogen compound solid electrolytes are disordered amorphous phases, containing a small amount of crystalline phases, which are residual raw materials Li2S or LiCl / NaCl.

[0172] like Fig.12 As shown, the crystal structure of the Li2S@ZrCl4 sulfur-halide compound solid electrolyte synthesized in Example 4 evolves with the ball milling time. The Li2S phase gradually disappears and reappears, and the LiCl phase appears at the same time.

[0173] 3. Quantitative analysis of phase

[0174] (1) Characterization methods

[0175] In an argon atmosphere glove box without water or oxygen, the solid electrolyte powders prepared in Examples 1-3 and Comparative Example 1 were uniformly mixed with a silicon powder standard sample at a mass ratio of 9:1, and the obtained mixed samples were characterized using an X-ray diffractometer. The XRD pattern of the obtained mixed sample was fitted to obtain the amorphous phase content.

[0176] (2) Characterization results

[0177] The amorphous phase content of various halide solid electrolytes was obtained from the XRD patterns after mixing with the standard samples, as shown in Table 2.

[0178] Table 2 Amorphous phase content of halide solid electrolyte

[0179] sample Amorphous phase content <![CDATA[Li2ZrCl6 (Comparative Example 1)]]> 32% <![CDATA[Li2O@ZrCl4 (Example 1)]]> 88% <![CDATA[Li2S@ZrCl4 (Example 1)]]> 76% <![CDATA[Li3N@ZrCl4 (Example 1)]]> 74% <![CDATA[Na2S@ZrCl4 (Example 2)]]> 72% <![CDATA[Ag2O@ZrCl4 (Example 3)]]> 68%

[0180] 4. Microstructure characterization and analysis

[0181] (1) Characterization methods

[0182] The microstructure of the halide solid electrolyte synthesized in Example 1 was characterized using high-resolution cryo-transmission electron microscopy.

[0183] The EDS surface scan of the Na2S@ZrCl4 sulfur-halide compound solid electrolyte synthesized in Example 6 was characterized using a high-resolution cryo-transmission electron microscope.

[0184] (2) Characterization results

[0185] The characterization results are as follows Figure 3 As shown, the results show that the halide solid electrolyte is mostly a disordered amorphous phase, with a small amount of crystalline phase embedded in the amorphous matrix. The crystalline phase is LiCl, and the grain size is about 10nm.

[0186] Crystal structure characterization analysis and microstructure characterization analysis show that lithium salts with different anions (oxygen ions, sulfur ions, nitrogen ions) react with ZrCl4 to obtain materials with similar crystal structures and microstructures, and have high ionic conductivity. This solid-phase reaction behavior is similar to the dissociation behavior of salt in solution, which can be understood as the dissociation behavior of lithium salt (solute) in ZrCl4 (solid solvent).

[0187] The characterization results are as follows Fig.13 As shown, the results show that the sulfur-halide compound solid electrolyte is small particles of hundreds of nanometers, and the Na, S, Zr, and Cl elements are evenly distributed.

[0188] 2. Electrochemical performance test

[0189] 1. Constant current charge and discharge test

[0190] (1) Test method

[0191] At room temperature, the all-solid-state batteries provided in Examples 10-12 were subjected to constant current charge and discharge tests using a blue battery test system, wherein the voltage range for testing the samples of Examples 10 and 11 was 2.5 V to 4.3 V (relative to Li + The voltage range of the test of the sample of Example 12 is 1.5V to 4.0V. The first 3 cycles are activated at a rate of 0.3C. From the 4th cycle onwards, a rate of 1C is used. The charge and discharge curves of the first and second cycles of the all-solid-state batteries provided in Examples 10 and 11 are shown in Figures 1 and 2, respectively. Figure 6 and Figure 8 The charge and discharge curve of the second cycle of the all-solid-state battery provided in Example 6 is shown in Fig. 9 .

[0192] At room temperature, the all-solid-state battery provided in Example 14 was subjected to constant current charge and discharge tests using a blue battery test system, with a voltage range of 2.5 V to 4.3 V (relative to Li + / Li voltage), and the first 3 cycles were performed at a rate of 0.1C.

[0193] (2) Test results

[0194] Test results such as Figure 6 , Figure 8 , Fig. 9 shown.

[0195] The all-solid-state battery provided in Example 10 has no obvious polarization at a rate of 0.3C, and has a high first-cycle coulomb efficiency (86.3%) and reversible capacity (193 mAh g -1 ).

[0196] The all-solid-state battery provided in Example 11 has no obvious polarization at a rate of 0.3C and has a high reversible capacity (176 mAh g -1 ).

[0197] The all-solid-state battery provided in Example 12 has no obvious polarization at a rate of 0.3C and has a high reversible capacity (163 mAh g -1 ).

[0198] Test results such as Fig.14 shown.

[0199] The all-solid-state battery provided in Example 14 has a reversible capacity of 195.6 mAh g at a rate of 0.1 C. -1 , with an efficiency of 83.8% in the first week.

[0200] 2. Cycle rate performance test

[0201] (1) Test method

[0202] At room temperature, the blue battery test system was used to test the cycle performance of the all-solid-state battery provided in Example 13, and the voltage range was 2.5V to 4.3V (relative to Li + / Li voltage), the first 3 cycles were activated at a rate of 0.3C, and from the 4th cycle onwards, a rate of 1C was used.

[0203] (2) Test results

[0204] The specific capacity-cycle number graph for the first 100 cycles is shown in the figure below: Figure 7 As shown in the results, the reversible capacity of the 4th cycle (1C rate) is about 152 mAh g -1 After 100 cycles, the capacity retention rate is 94%.

[0205] Figure 6 and Figure 7 The battery performance results show that the all-solid-state lithium battery assembled using Li2O@ZrCl4 halide solid electrolyte has excellent high capacity and cycle stability at room temperature.

[0206] 3. Low temperature service performance test

[0207] (1) Test method

[0208] At low temperature (-30°C), the all-solid-state battery provided in Example 13 was subjected to constant current charge and discharge tests using the Blue Electric Battery Test System. The voltage range was 2.5V to 4.3V (voltage relative to Li+ / Li). The first three cycles were activated at a rate of 0.1C, and from the fourth cycle onwards, a rate of 1C was used.

[0209] (2) Test results

[0210] The results are as follows Fig.10 As shown, the results show that the assembled all-solid-state battery still has 110 mAh g at low temperature (-30 ° C). -1 The specific capacity and capacity retention rate after 80 stable cycles are 99%, indicating its excellent low-temperature performance.

[0211] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A composite halide solid electrolyte, characterized in that: The structural formula of the composite halide solid electrolyte is: a B b ) m @(MX c ) n ,in: A represents that the general structural formula contains at least one of Li, Na, K, Cu and Ag; B indicates that the general structural formula contains S 2- OH - NH 2- 、O2 2- , O 2- and N 3- At least one of M represents that the general structural formula contains at least one of Zr, Hf, Ta, Nb, Al, Fe and Ga; X represents that the general structural formula contains at least one of F, Cl, Br and I; a and b represent A a B b The corresponding number of atoms in the compound, c represents MX c The corresponding number of atoms in the compound; m and n represent A a B b Compounds and MX c The amount of substance in a compound.

2. The composite halide solid electrolyte according to claim 1, characterized in that The structural formula of the composite halide solid electrolyte is: a B b ) m @(MX c ) n , where: M indicates that the general structural formula contains Zr, and c is 4.

3. The composite halide solid electrolyte according to claim 1, characterized in that: The structural formula of the composite halide solid electrolyte is: a B b ) m @(MX c ) n , where: B means that the general structure contains S 2- , a is 2, b is 1.

4. The composite halide solid electrolyte according to claim 3, characterized in that: Also includes additive A x Z; Z means containing O2 - 、CO3 2- PO4 3- 、P2O7 4- 、SO4 2- At least one of the following; x represents a positive integer from 1 to 4.

5. The composite halide solid electrolyte according to claim 1, characterized in that: The composite halide solid electrolyte comprises an amorphous phase and a crystalline phase, wherein the crystal grains of the crystalline phase are embedded in the matrix of the amorphous phase; the chemical composition of the crystalline phase comprises AX, and the constituent ions of the amorphous phase comprise A, B, M, and X.

6. The composite halide solid electrolyte according to claim 1, characterized in that: Raw materials include A a B b and MX c ; Among them, A a B b and MX c The amount of substance ratio is 0.3:1 to 3:

1.

7. The composite halide solid electrolyte according to claim 6, characterized in that Raw material A a B b Including at least one of lithium hydroxide, sodium hydroxide, lithium amide, sodium amide, lithium peroxide, sodium peroxide, lithium oxide, sodium oxide, silver oxide, cuprous oxide, lithium sulfide, sodium sulfide, silver sulfide, cuprous sulfide and lithium nitride; and / or, raw material MX c The invention comprises at least one of anhydrous zirconium tetrafluoride, anhydrous zirconium tetrachloride, anhydrous zirconium tetrabromide, anhydrous zirconium tetraiodide, anhydrous tantalum pentachloride and anhydrous silicon chloride.

8. A method for preparing a composite halide solid electrolyte, characterized in that: The following steps are involved: In an inert atmosphere without water or oxygen, raw material A a B b and MX c The composite halide solid electrolyte (A) was obtained by mechanical ball milling to produce a solid phase reaction. a B b ) m @(MX c ) n .

9. The method for preparing the composite halide solid electrolyte according to claim 8, characterized in that: Mechanical ball milling control parameters include: The grinding beads are one or more of grinding beads with a diameter of 3 mm to 10 mm; and / or the total mass ratio of grinding beads to raw materials is 60:1 to 20:1; And / or the ball milling time is 3h to 80h; the ball mill speed is 400r / min to 800r / min.

10. A battery, characterized in that: A composite halide solid electrolyte comprising the composite halide solid electrolyte according to any one of claims 1 to 7, or a composite halide solid electrolyte obtained by the preparation method according to any one of claims 8 to 9.

Citation Information

Cited By

  • Tantalum oxide co-doped aluminum-based oxyhalide solid electrolyte as well as preparation method and application thereof

    CN121748509A

  • Sulfide solid electrolyte, preparation method and all-solid-state lithium ion battery

    CN121839853A

  • Solid electrolyte and preparation method therefor, and battery

    WO2026026595A1