Method for manufacturing non-aqueous secondary battery and device for manufacturing non-aqueous secondary battery

By adopting the lamination process, the concave and convex forming process and the pressure planarization process in the manufacturing process of non-aqueous secondary batteries, the problem of deformation of the electrode laminate is solved, the uniform thickness and high density of the electrode layer are achieved, and the performance of the battery is improved. .

CN118738583APending Publication Date: 2024-10-01HONDA MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410214969.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the conventional technology, it is difficult to obtain an electrode laminate with a uniform thickness when manufacturing a non-aqueous secondary battery, and the widthwise deformation of the laminate during roll rolling cannot be sufficiently suppressed.

Method used

The positive electrode layer and the electrolyte layer are laminated in a lamination process. In the unevenness forming process, pressure is applied to the surface and thickness directions of the laminate to form uneven areas. The uneven areas are then flattened in the pressure planarization process, using the protrusion of the pressing member. The laminated body is partially contacted to locally increase the stress, the contact area is reduced to increase the density, and heating is performed to homogenize the temperature before the unevenness forming process.

Benefits of technology

It effectively suppresses the deformation of the laminated body, improves the density and homogeneity of the electrode layer, reduces the displacement and warpage in the width direction, and improves the performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738583A_ABST
    Figure CN118738583A_ABST
Patent Text Reader

Abstract

The problem to be solved by the present invention is to provide a method for manufacturing a non-aqueous secondary battery capable of suppressing deformation of a laminate. In order to solve the problem, the present invention provides a method for manufacturing a nonaqueous secondary battery, the method comprising, in the following order: a lamination step for obtaining a laminate by laminating a positive electrode layer containing a positive electrode active material and an electrolyte layer containing a solid electrolyte; a step for forming recesses and / or protrusions extending from one side toward the other side while applying pressure in the thickness direction of the laminate from the one side toward the other side in the surface direction of the laminate; and a pressure planarization step for planarizing the concave portions and / or the convex portions while applying pressure in the thickness direction to the laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a non-aqueous secondary battery and a device for manufacturing a non-aqueous secondary battery. Background Art

[0002] In recent years, research and development related to secondary batteries that contribute to energy efficiency have been conducted in order to ensure that more people have access to affordable, reliable, sustainable and advanced energy.

[0003] As such secondary batteries, non-aqueous secondary batteries such as lithium ion secondary batteries in which an electrolyte layer is disposed between a positive electrode layer and a negative electrode layer are known. Such non-aqueous secondary batteries are pressurized by a method such as roll pressing in order to increase density during the manufacturing process.

[0004] For example, a method for manufacturing a positive electrode plate can suppress the occurrence of poor shape of a positive electrode plate precursor and the falling off of a positive electrode active material mixture during roller rolling, and can uniformly increase the filling density of the positive electrode active material mixture. As the aforementioned method for manufacturing the positive electrode plate, a method for roller rolling a positive electrode plate precursor using an embossing roller pair having a pair of embossing rollers is disclosed (for example, refer to patent document 1).

[0005] [Prior Technical Literature]

[0006] (Patent Document)

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 9-204915 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] The technology disclosed in Patent Document 1 is to use an embossing roller to roll the positive plate precursor in two stages to suppress the occurrence of poor shape of the positive plate precursor and the shedding of the positive electrode active material mixture during roll rolling. However, when the above method is applied to an electrode stack, an electrode stack with uniform thickness cannot be obtained, and deformation in the width direction of the stack during roll rolling cannot be fully suppressed.

[0010] The present invention has been made in view of the above, and an object of the present invention is to provide a method for manufacturing a non-aqueous secondary battery that can suppress deformation of a stacked body.

[0011] [Technical means to solve the problem]

[0012] (1) The present invention relates to a method for manufacturing a non-aqueous secondary battery, which comprises, in sequence: a stacking step, in which a positive electrode layer containing a positive electrode active material and an electrolyte layer containing a solid electrolyte are stacked to obtain a stacked body; a concave-convex forming step, in which a pressure is applied from one side of the surface direction of the stacked body toward the other side in the thickness direction of the stacked body to form a concave portion and / or a convex portion extending from the one side toward the other side; and a pressurized flattening step, in which a pressure is applied to the stacked body in the thickness direction to flatten the concave portion and / or the convex portion.

[0013] According to the invention of (1), a method for producing a non-aqueous secondary battery capable of suppressing deformation of a stacked body can be provided.

[0014] (2) A method for manufacturing a non-aqueous secondary battery according to (1), wherein, in the aforementioned concave-convex forming step, a pressurizing member having a protrusion protruding from a base is brought into contact with the aforementioned stacked body to apply pressure, thereby forming the aforementioned concave portion and / or the aforementioned convex portion on the aforementioned stacked body, and at this time, only the aforementioned protrusion of the aforementioned pressurizing member contacts the aforementioned stacked body.

[0015] According to the invention of (2), the contact area between the pressurizing member and the stacked body is reduced, and the stress can be locally increased, so that it is easy to increase the density of the portion where the protrusion contacts the stacked body.

[0016] (3) The method for producing a nonaqueous secondary battery according to (1) or (2), further comprising a heating step of heating the stacked body before the unevenness forming step.

[0017] According to the invention of (3), the temperature unevenness of the laminate can be reduced during the unevenness forming step, so the homogeneity of the laminate accompanying the pressurization can be improved.

[0018] (4) A method for manufacturing a non-aqueous secondary battery according to any one of (1) to (3), wherein the aforementioned concavo-convex forming step and the aforementioned pressurized flattening step are performed by clamping the aforementioned stack through a roller, and the diameter of the roller used in the aforementioned pressurized flattening step is larger than the diameter of the roller used in the aforementioned concavo-convex forming step.

[0019] According to the invention of (4), the concave and / or convex parts can be easily and precisely processed in the concave-convex forming step, so the accuracy of the concave and / or convex parts can be improved. In addition, the curvature of the roller in the pressurizing and flattening step can be made close to flat and pressurized uniformly, so the deformation caused by the undulation of the laminate can be further suppressed.

[0020] (5) In addition, the present invention relates to a manufacturing device for a non-aqueous secondary battery, which comprises: a stacking section for stacking a positive electrode layer containing a positive electrode active material and an electrolyte layer containing a solid electrolyte to obtain a stacked body; a concave-convex forming section for applying pressure from one side of the surface direction of the stacked body toward the other side along the thickness direction of the stacked body to form concave portions and / or convex portions extending from the one side toward the other side; and a pressurized flattening section for flattening the concave portions and / or convex portions while applying pressure in the thickness direction to the stacked body.

[0021] According to the invention of (5), the manufacturing method of (1) can be carried out.

[0022] (6) The non-aqueous secondary battery manufacturing apparatus according to (5), wherein the concavo-convex forming section and the pressurizing and flattening section have rollers for clamping and conveying the stacked body, and the diameter of the roller of the pressurizing and flattening section is larger than the diameter of the roller of the concavo-convex forming section.

[0023] According to the invention of (6), the manufacturing method of (4) can be carried out. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a diagram showing the structure of a non-aqueous secondary battery manufacturing apparatus according to one embodiment of the present invention.

[0025] Figure 2 This is a diagram showing a concavo-convex formation portion according to one embodiment of the present invention.

[0026] Figure 3 This is a diagram showing the structure of a laminated body according to one embodiment of the present invention.

[0027] Figure 4 The figure shows the simulation result of forming the concavities and convexities on the laminated body by the manufacturing method of the non-aqueous secondary battery of the present invention. DETAILED DESCRIPTION

[0028] [Non-aqueous secondary battery]

[0029] Examples of the nonaqueous secondary battery manufactured by the method for manufacturing a nonaqueous secondary battery according to the present embodiment include a semisolid lithium ion battery having a gel electrolyte and an all-solid lithium ion battery having a solid electrolyte.

[0030] The non-aqueous secondary battery of this embodiment has a stacked body S in which electrode layers and electrolyte layers disposed therebetween are stacked. The stacked body S is, for example, Figure 3 As shown, it has a negative electrode layer S1, a positive electrode layer S2 and an electrolyte layer S3 disposed between these layers. Figure 3Illustrates the structure of the laminate of the finally manufactured non-aqueous secondary battery. The laminate, which is the object for forming recesses and / or protrusions by the uneven formation process, which is one process of the manufacturing method of the non-aqueous secondary battery of the present embodiment, will be described below.

[0031] (Positive electrode layer)

[0032] The positive electrode layer S2 has a positive electrode active material layer S21 and a positive electrode current collector S22. In the present embodiment, the positive electrode active material layer S21 is laminated on both sides of the positive electrode current collector S22. In addition, the structure of the positive electrode layer S2 is not limited to the above, and the positive electrode active material layer may be laminated on a single side of the positive electrode current collector.

[0033] The positive electrode active material layer 21 is a layer that must contain a positive electrode active material. The positive electrode active material is not particularly limited, and a material known as a positive electrode active material for a non-aqueous secondary battery can be used. As the positive electrode active material, for example, ternary cathode materials such as LiCoO2, LiNiO2, NCM (Li(NixCoyMnz)O2, (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), layered positive electrode active material particles such as LiVO2, LiCrO2, spinel-type positive electrode active materials such as LiMn2O4, Li(Ni 0.25 Mn 0.75 )2O4, LiCoMnO4, Li2NiMn3O8, olivine-type positive electrode active materials such as LiCoPO4, LiMnPO4, LiFePO4, etc. can be used.

[0034] The positive electrode active material layer S21 may also contain a solid electrolyte, a conductive additive, a binder, etc. in addition to the positive electrode active material. The solid electrolyte, the conductive additive, the binder, etc. are not particularly limited, and materials known as electrode materials for non-aqueous secondary batteries can be applied.

[0035] The positive electrode current collector S22 is not particularly limited, and a material known as a positive electrode current collector for a non-aqueous secondary battery can be used. As the positive electrode current collector S22, for example, metal foils such as stainless steel (SUS) foil and aluminum (Al) foil can be cited.

[0036] (Electrolyte layer)

[0037] The electrolyte layer S3 is a layer disposed between the negative electrode layer S1 and the positive electrode layer S2 and must contain a solid electrolyte. In the electrolyte layer, in addition to the above, a binder, etc. may also be contained.

[0038] As the solid electrolyte, there is no particular limitation, and sulfide-based solid electrolytes, oxide-based solid electrolytes, nitride-based solid electrolytes, halide-based solid electrolytes, etc. can be cited.

[0039] (Negative electrode layer)

[0040] The negative electrode layer S1 includes a negative electrode active material layer S11 and a negative electrode current collector S12. In the present embodiment, the negative electrode active material layer S11 is stacked so as to be in contact with the electrolyte layer S3.

[0041] The negative electrode active material layer S11 is a layer that must contain a negative electrode active material. The negative electrode active material is not particularly limited, and a material known as a negative electrode active material for a non-aqueous secondary battery can be used. Examples of the negative electrode active material include lithium titanate (Li4Ti5O 12 ) and other lithium transition metal oxides, transition metal oxides such as TiO2, Nb2O3 and WO3, metal sulfides, metal nitrides, graphite, carbon materials such as soft carbon and hard carbon, silicon materials such as silicon monomers, silicon alloys, silicon compounds, as well as lithium metal, lithium alloys and metal indium.

[0042] The negative electrode active material layer S11 may contain, in addition to the negative electrode active material, a solid electrolyte, a conductive aid, a binder, etc. The solid electrolyte, conductive aid, binder, etc. are not particularly limited, and any known material as an electrode material for a non-aqueous secondary battery may be used.

[0043] The negative electrode current collector S12 is not particularly limited, and any known negative electrode current collector for non-aqueous secondary batteries can be used. Examples of the negative electrode current collector include metal foils such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.

[0044] <Method for producing non-aqueous secondary battery>

[0045] The manufacturing method of a non-aqueous secondary battery sequentially comprises: a stacking step to obtain a stacked body having at least a positive electrode layer and an electrolyte layer stacked thereon; a concave-convex forming step to form concave portions and / or convex portions on the stacked body obtained above; and a pressurized flattening step to flatten the concave portions and / or convex portions. In addition, each of the above steps is at least a part of the steps of the manufacturing method of a non-aqueous secondary battery, and the manufacturing method of a non-aqueous secondary battery of this embodiment may also include steps other than the above. For example, a heating step of heating the entire stacked body obtained by the stacking step may also be included between the stacking step and the concave-convex forming step.

[0046] The stacking process is a process of stacking at least a positive electrode layer and an electrolyte layer. The stacking process may also be a process of stacking sheet-shaped positive electrode layers and electrolyte layers that are separately formed. In addition to the above, the stacking process may also be a process of applying an electrolyte layer slurry containing materials constituting the electrolyte layer on the positive electrode layer and drying it, or may be a process of applying a positive electrode layer slurry containing materials constituting the positive electrode layer on the electrolyte layer and drying it. There is no particular limitation on the method of applying and drying, and a method known as a method for manufacturing a non-aqueous secondary battery may be applied. In addition to the above, the stacking process may also be a process of stacking a positive electrode layer, an electrolyte layer and a negative electrode layer.

[0047] The heating process is a process for heating the entire laminate obtained by the lamination process. By the heating process, the unevenness of the temperature of the laminate can be reduced, so the homogeneity of the laminate can be improved in the concave-convex forming process. There is no particular limitation on the method of heating the laminate by the heating process, and a method based on a known heating device such as a ceramic heater, a sheath heater, a halogen lamp heater, an induction heater, etc. can be applied.

[0048] The concavoconvex forming process is a process for forming concave and / or convex portions on the laminate obtained by the lamination process. In the concavoconvex forming process, while applying pressure along the thickness direction of the laminate from one side of the surface direction of the laminate toward the other side, concave and / or convex portions are formed on the laminate. As a result, concave and / or convex portions extending from the above-mentioned one side of the laminate toward the other side are formed. That is, the direction in which pressure is applied to the laminate in the concavoconvex forming process is the same as the direction in which the formed concave and / or convex portions extend. When the laminate is pressurized to perform high density, if the thickness direction is simply pressurized uniformly without the concavoconvex forming process, displacement (undulation) may sometimes occur in the width direction of the laminate, and thus warping of the laminate may occur. By sequentially performing the concavoconvex forming process and the pressurized flattening process, displacement in the width direction of the above-mentioned laminate can be suppressed.

[0049] The shape of the concave and / or convex portion formed by the concave-convex forming step is not particularly limited, and for example, a convex portion is formed between concave portions formed in a groove shape or a dot shape. In the above case, the shape of the concave portion may be a square shape, a wedge shape, a semicircular shape, or a combination of the above shapes when viewed in cross section, but is not particularly limited to the above shapes. The concave and / or convex portion is preferably formed uniformly in the width direction of the laminate.

[0050] The concavoconvex forming step is, for example, to sandwich the laminate through Figure 1 and Figure 2 The pressing is performed between the rollers of a roller pressing device 2 having a pair of rollers 20 and 21 as a pressing member as shown. Figure 1and Figure 2 In the embodiment, the thickness direction of the laminate is represented by the Z direction. The direction in which pressure is applied to the laminate in the concavo-convex forming step, i.e., the direction from one side of the surface direction of the laminate toward the other side, is represented by the X direction. The width direction of the laminate is represented by the Y direction. The pressure member is not limited to the pair of rollers described above, and may be, for example, a single roller. The following describes a structure in which the pressure member is a pair of rollers 20, 21.

[0051] The roller 20 as the pressing member is as follows Figure 2 As shown, there is a protrusion 20a protruding from the base in the Z direction. The protrusion 20a is formed along the circumference of the roller 20. A plurality of protrusions 20a may be formed in the Y direction. When a plurality of protrusions 20a are formed, a recessed portion 20b is formed between the protrusions 20a. The protrusion 20a of the roller 20 contacts the laminate S and presses the roller 20 in the Z direction, thereby forming a recessed portion Sa on the laminate S. When a plurality of protrusions 20a are formed, in the laminate S, the recessed portions Sa become convex portions Sb between each other.

[0052] Figure 4 FIG. 2 is a diagram showing the simulation result of stress distribution when the laminate S is pressurized by the roller having the protrusion as the pressurizing member. The simulation is performed by the finite element method. Figure 4 As shown, it can be seen that the portion with low stress extends toward the X direction, and a concave portion and / or a convex portion extending from one direction to the other direction is formed in the stacked body S.

[0053] exist Figure 2 , a structure in which a protrusion 20a is formed on a roller 20 disposed on the upper part of the stack S is shown, and preferably, a similar protrusion is also formed on a roller 21 disposed on the lower part of the stack S. That is, in the concavo-convex forming step, it is preferable to form concave portions and / or convex portions on both surfaces of the stack S. By forming concave portions and / or convex portions on both surfaces of the stack S, deformation such as warping of the stack S can be further suppressed.

[0054] It is preferred that when the roller 20 is brought into contact with the laminate S to apply pressure, Figure 2 As shown, only the protrusion 20a contacts the laminate S. That is, it is preferred that the bottom surface of the recessed portion 20b does not contact the laminate S. As a result, the contact area between the roller 20 and the laminate S is reduced, and stress is concentrated on the protrusion 20a, so the density of the laminate S at the recessed portion Sa can be further increased. When the same protrusion as that of the roller 20 is formed on the roller 21, it is preferred that the positions of the protrusions of the roller 21 and the roller 20 in the X direction and the Y direction are consistent when the laminate S is pressed. As a result, the density of the laminate S at the recessed portion can be further increased.

[0055] The pressurized flattening process is a process of pressurizing the laminate S to flatten the concave and / or convex portions of the laminate S formed with concave and / or convex portions by the concave-convex forming process to make the thickness uniform. The pressurized flattening process is used to uniformly densify the laminate S. In the pressurized flattening process, stress is concentrated on the thick portion of the laminate S to flatten it. At this time, if the thick portion of the laminate S (for example, Figure 2 If the convex portion Sb in the stack is crushed, it can retreat to a thin portion of the stack S (for example, Figure 2 Thus, compared with the case where the concavo-convex forming step is not provided, the extension of the stacked body S in the Y direction is reduced, and the undulation of the stacked body S is suppressed.

[0056] The pressurized flattening process is performed by, for example, clamping the laminate through Figure 1 The flattening step is performed between the rollers in the rolling device 3 having a pair of rollers as shown in the figure. The surface of the roller in the rolling device 3 that contacts the laminate is a flat surface, and no protrusion is formed. The specific method of the pressurization flattening step is not limited to the method using a pair of rollers as described above, and for example, it may be a method based on a single roller or a method based on a flat press.

[0057] In borrowing Figure 1 When the roller pressing device 3 as shown in the figure performs the pressurizing and flattening process, the diameter R3 of the roller of the roller pressing device 3 is preferably larger than the diameter R2 of the roller of the roller pressing device 2 performing the concavo-convex forming process. As a result, the curvature of the roller of the roller pressing device 3 becomes smaller, so that the laminate S can be pressed more uniformly, and the deformation caused by the undulation of the laminate S can be further suppressed. In addition, since the diameter R2 of the roller of the roller pressing device 2 is smaller than the diameter R3 of the roller of the roller pressing device 3, the concave and / or convex portions of the laminate S can be accurately and easily formed.

[0058] The laminated body in which the concave and / or convex portions are formed by the above-mentioned concave-convex forming step and the concave and convex portions are flattened by the pressurizing flattening step can be a laminated body in which at least a positive electrode layer and an electrolyte layer are stacked. Figure 3 A laminated body having a positive electrode layer, an electrolyte layer, and a negative electrode layer laminated as shown.

[0059] <Non-aqueous secondary battery manufacturing device>

[0060] The non-aqueous secondary battery manufacturing apparatus 100 for executing the non-aqueous secondary battery manufacturing method is as follows: Figure 1 As shown, the laminating unit 1, a roll pressing device 2 as a concavo-convex forming unit, and a roll pressing device 3 as a pressurizing and flattening unit are provided. Figure 1The above is an example, and the manufacturing apparatus 100 may be an apparatus that stacks sheets Sx and Sy and presses them by a roller press.

[0061] The laminated part 1 is, for example, Figure 1 As shown, a sheet Sx including a positive electrode layer formed in a sheet shape and a sheet Sy including an electrolyte layer formed in a sheet shape are stacked by a stacking roller. The structure of the stacking unit 1 is not limited to the above, and can be composed of a coating device that coats the positive electrode layer slurry and the electrolyte layer slurry on the pre-formed sheet Sx or sheet Sy, or a combination of the above.

[0062] The structure of the roller pressing device 2 as the concavo-convex forming part is as described in the description of the concavo-convex forming step. For example, the roller pressing device 2 includes a pair of rollers arranged above and below in the thickness direction of the laminate. At least one of the rollers is formed with a protrusion. By passing the laminate through the pair of rollers, a concave portion and / or a convex portion is formed on the laminate. The structure of the concavo-convex forming part is not limited to the above, and for example, it may be a device having one roller.

[0063] The structure of the roller pressing device 3 as the pressurizing and flattening section is as described in the above description of the pressurizing and flattening step. The roller pressing device 3 includes, for example, a pair of rollers arranged above and below in the thickness direction of the laminate. The surfaces of the pair of rollers in contact with the laminate are flat and no protrusions are formed. The structure of the pressurizing and flattening section is not limited to the above, and may be, for example, a device including one roller or a flat pressing device.

[0064] As mentioned above, although the preferred embodiment of the present invention has been described, the present invention is not limited to the above-mentioned embodiment, and modifications and improvements within the scope that can achieve the object of the present invention are included in the present invention.

[0065] Reference numerals

[0066] 100Non-aqueous secondary battery manufacturing device

[0067] 1Lamination section

[0068] 2Concave-convex forming part

[0069] 3 Pressurized flattening section

[0070] S laminate

Claims

1. A method for manufacturing a non-aqueous secondary battery, comprising: A lamination step of laminating a positive electrode layer including a positive electrode active material and an electrolyte layer including a solid electrolyte to obtain a laminate; a concavo-convex forming step of forming a concave portion and / or a convex portion extending from one side toward the other side in the surface direction of the laminate while applying pressure in the thickness direction of the laminate; and The pressure planarization step planarizes the concave portion and / or the convex portion while applying pressure in the thickness direction of the stacked body.

2. The method for manufacturing a non-aqueous secondary battery according to claim 1, wherein: In the above-mentioned concave-convex forming step, a pressurizing member having a protrusion protruding from a base is brought into contact with the above-mentioned stacked body and pressurized, thereby forming the above-mentioned concave portion and / or the above-mentioned convex portion on the above-mentioned stacked body. At this time, only the above-mentioned protrusion of the above-mentioned pressurizing member contacts the above-mentioned stacked body.

3. The method for manufacturing a non-aqueous secondary battery according to claim 1 or 2, wherein: A heating step of heating the laminated body is provided before the concavo-convex forming step.

4. The method for manufacturing a non-aqueous secondary battery according to claim 1 or 2, wherein: The above-mentioned concavo-convex forming step and the above-mentioned pressurized flattening step are performed by clamping the above-mentioned laminated body through rollers. The diameter of the roller used in the pressurizing and flattening step is larger than the diameter of the roller used in the unevenness forming step.

5. A non-aqueous secondary battery manufacturing device, comprising: A lamination unit for laminating a positive electrode layer including a positive electrode active material and an electrolyte layer including a solid electrolyte to obtain a laminate; A concave-convex forming portion, which forms a concave portion and / or a convex portion extending from one side toward the other side in the surface direction of the stacked body while applying pressure in the thickness direction of the stacked body from one side toward the other side; and, The pressurizing and flattening section flattens the concave portion and / or the convex portion while applying pressure in the thickness direction to the stacked body.

6. The manufacturing apparatus for a non-aqueous secondary battery according to claim 5, wherein: The concavoconvex forming section and the pressurizing and flattening section have rollers for sandwiching and conveying the laminated body. The diameter of the roller of the pressurizing and flattening portion is larger than the diameter of the roller of the unevenness forming portion.