Solid electrolyte membrane and preparation method thereof and battery

By using a two-layer solid electrolyte membrane in solid-state batteries, lithium-philic materials are used to alloy lithium metal with lithium metal to form a highly dense alloy layer and negative electrode active material to improve lithium ion deposition, which solves the problem of lithium dendrites growth in lithium metal batteries. Short circuit problem achieves more stable cycle performance and safety.

CN118738609BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411218603.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

When lithium metal is used as the negative electrode in an all-solid-state battery, dendrites are very likely to grow along the pores and cracks of the electrolyte layer, resulting in short-circuit problems. The prior art is difficult to effectively suppress the growth of lithium dendrites and the density of the electrolyte layer.

Method used

A solid electrolyte membrane adopts a double-layer structure, wherein the first solid electrolyte layer conducts active ions and isolates electrons, and the second solid electrolyte layer consists of lithium-philic material and negative electrode active material, and the lithium-philic material is alloyed with lithium metal to form a high density The alloy layer inhibits the growth of lithium dendrites and improves lithium ion deposition uniformity through the negative electrode active material.

Benefits of technology

Effectively inhibit the growth of lithium dendrites, avoid short circuits, improve the cycle stability and rate performance of lithium metal batteries, and improve the safety and working life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738609B_ABST
    Figure CN118738609B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and in particular to a solid electrolyte membrane, a preparation method thereof, and a battery. The solid electrolyte membrane provided comprises a first solid electrolyte layer and a second solid electrolyte layer disposed on the surface of the first solid electrolyte layer; the first solid electrolyte layer comprises a first solid electrolyte; the second solid electrolyte layer comprises a second solid electrolyte, a lithium-philic material, and a negative electrode active material, wherein the lithium-philic material is selected from a material suitable for alloying with lithium metal to form a lithium alloy, and the negative electrode active material comprises lithium titanate and / or a carbon material. The present application can alleviate the problem that lithium metal can easily grow along the pores and cracks of the electrolyte layer and thus cause a short circuit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a solid electrolyte membrane and a preparation method thereof, and a battery. Background Art

[0002] Compared with traditional lithium-ion batteries, solid-state batteries can avoid safety hazards caused by electrolyte leakage and other problems because there is no electrolyte inside. In addition, solid-state lithium batteries have attracted widespread attention from researchers due to their high energy density, good safety performance, and no memory effect. Metallic lithium is considered to be one of the better choices for high-energy-density battery negative electrode materials because of its ultra-high theoretical specific capacity density and low reduction potential. However, the uneven deposition of lithium ions on the lithium metal negative electrode will cause the growth of lithium dendrites, that is, the growth of lithium dendrites and the short circuit caused by the existence of lithium dendrites restrict the practical application of metal lithium negative electrodes.

[0003] All-solid-state electrolytes are considered to be one of the effective ways to solve the problem of dendrite growth in lithium metal negative electrodes due to their high hardness. However, a large number of experimental results show that when lithium metal is used as the negative electrode in an all-solid-state battery, dendrites can easily grow along the pores and cracks between the electrolytes and eventually cause a short circuit. In order to alleviate this problem, the relevant technology proposes to inhibit the growth of lithium dendrites by doping a small amount of metal in the double-layer electrolyte. However, the porosity of the electrolyte layer prepared in this way is still high after molding, and the doped metal material will also increase the electronic conductivity of the electrolyte layer, increasing the possibility of lithium metal deposition inside the electrolyte.

[0004] In view of this, this application is hereby filed. Summary of the invention

[0005] In view of this, the present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the present invention provides a solid electrolyte membrane and a preparation method thereof and a battery, which can alleviate the problem that lithium metal easily grows along the pores and cracks of the electrolyte layer and causes a short circuit.

[0006] In order to solve the above technical problems, this application is implemented as follows:

[0007] According to one aspect of the present application, an embodiment of the present application provides a solid electrolyte membrane, the solid electrolyte membrane comprising a first solid electrolyte layer and a second solid electrolyte layer disposed on a surface of the first solid electrolyte layer;

[0008] The first solid electrolyte layer includes a first solid electrolyte;

[0009] The second solid electrolyte layer includes a second solid electrolyte, a lithium-philic material and a negative electrode active material, wherein the lithium-philic material is selected from materials suitable for alloying with lithium metal to form a lithium alloy, and the negative electrode active material includes lithium titanate and / or a carbon material.

[0010] In addition, the solid electrolyte membrane according to the present application may also have the following additional technical features:

[0011] In some embodiments, the lithium insertion potential of the lithiophilic material is ≥0.3V.

[0012] In some embodiments, the volume expansion rate of the lithium-philic material after alloying with lithium metal to form a lithium alloy is ≥50%.

[0013] In some embodiments, the lithium-philic material comprises Si, SiO x , SiC, Ge, Sn, Al, In, Mg, Sb, Zr, Mn, Ce, Y, La or Sc, wherein x ≥ 0.5.

[0014] In some embodiments, the average particle size of the lithiophilic material is 0.01 μm to 100 μm.

[0015] In some of the embodiments, the carbon material includes at least one of graphite, hard carbon or soft carbon.

[0016] In some embodiments, the first solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte, or lithium nitride.

[0017] In some embodiments, the second solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte or lithium nitride.

[0018] In some embodiments, the mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is (10-50): (50-80): (10-20).

[0019] In some embodiments, the first solid electrolyte layer further includes a first binder, and the mass fraction of the first binder in the first solid electrolyte layer is 2% to 10%.

[0020] In some embodiments, the second solid electrolyte layer further includes a second binder, and the mass fraction of the second binder in the second solid electrolyte layer is 2% to 10%.

[0021] In some embodiments, the thickness of the first solid electrolyte layer is 5 μm to 100 μm.

[0022] In some embodiments, the second solid electrolyte layer has a thickness of 5 μm to 100 μm.

[0023] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a solid electrolyte membrane as described above, the method comprising:

[0024] preparing a first solid electrolyte layer; and

[0025] forming a second solid electrolyte layer on the first solid electrolyte layer;

[0026] The method for preparing the first solid electrolyte layer comprises: mixing the first solid electrolyte, the first binder and the first solvent, and then homogenizing, coating and drying;

[0027] The method for forming the second solid electrolyte layer comprises: mixing a second solid electrolyte, a lithium-philic material, a negative electrode active material, a second binder and a second solvent, followed by homogenization, coating and drying.

[0028] According to another aspect of the present application, an embodiment of the present application provides a battery, the battery comprising a positive electrode, a negative electrode and the aforementioned solid electrolyte membrane or a solid electrolyte membrane prepared according to the aforementioned method;

[0029] The solid electrolyte membrane is arranged between the positive electrode and the negative electrode, the positive electrode is arranged close to the first solid electrolyte layer, and the negative electrode is arranged close to the second solid electrolyte layer.

[0030] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0031] In the embodiment of the present application, the solid electrolyte membrane provided includes a first solid electrolyte layer and a second solid electrolyte layer, wherein the second solid electrolyte layer includes a second solid electrolyte, a lithium-philic material and a negative electrode active material. Thus, the first solid electrolyte layer can be provided to conduct active ions such as lithium ions while isolating electronic conduction. In particular, the lithium-philic material and the negative electrode active material in the second solid electrolyte layer can inhibit lithium dendrites. The main mechanism of action is that the lithium-philic material can alloy with lithium metal to cause volume change and expansion, thereby producing a welding effect, fusing and compressing the pores with each other so that the second solid electrolyte layer is almost free of pores. At the same time, the high hardness makes it difficult to crack, and lithium dendrites cannot penetrate the second solid electrolyte layer, so that lithium dendrites can neither grow along the pores of the electrolyte nor pierce the second solid electrolyte layer, so that lithium metal can work stably; the addition of negative electrode active materials such as lithium titanate, carbon materials and other substances can induce uniform deposition of lithium ions and improve the physical contact between lithium metal and the second solid electrolyte layer, which has a positive significance for improving performance.

[0032] Therefore, the solid-state battery using the above-mentioned solid electrolyte membrane provided by the present application can effectively inhibit the growth of lithium metal dendrites, so that the solid-state battery such as the all-solid-state lithium metal battery can achieve long cycles without short circuits; the present application can make the performance of the solid-state battery more stable during the cycle process by improving the deposition uniformity of lithium metal.

[0033] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Shown is a graph of the first cycle charge and discharge data of the all-solid-state lithium metal battery prepared in Example 1 of the present invention (wherein the horizontal axis is the specific capacity and the vertical axis is the voltage).

[0035] Figure 2 Shown is a graph of cycle performance test data of the all-solid-state lithium metal battery prepared in Example 1 of the present invention (wherein the horizontal axis is the number of cycles and the vertical axis is the specific capacity). DETAILED DESCRIPTION

[0036] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.

[0037] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0038] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0039] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0040] As analyzed in the background technology, during the use of solid-state batteries with lithium metal as the negative electrode, the uneven deposition of lithium ions on the lithium metal negative electrode will cause the growth of lithium dendrites. In addition, although all-solid-state electrolytes are considered to be one of the effective ways to solve the problem of dendrite growth at lithium metal negative electrodes due to their high hardness; however, after a large number of experimental results, it is shown that when lithium metal is used as the negative electrode in all-solid-state batteries, dendrites are very easy to grow along the pores and cracks between the electrolytes and eventually cause short circuits. That is, since the solid electrolyte layer is not completely dense and there are pores in it, this will cause the solid electrolyte layer to be easily pierced by lithium dendrites during the cycle, which will cause the positive and negative electrodes of the solid-state battery to short-circuit due to the presence of lithium dendrites, causing battery failure and safety hazards. Most of the traditional methods for inhibiting the growth of lithium dendrites are to directly protect lithium metal, which has poor protection effect, or high cost, high risk, and long time consumption; and the present invention can effectively inhibit the growth of lithium dendrites by designing the composition and structure of the all-solid-state electrolyte membrane, avoiding its adverse effects on the lithium metal negative electrode, and has low process cost and low risk.

[0041] In view of this, based on the fact that the electrolyte still has a high porosity after pressurization in an all-solid-state battery system, and due to its brittle nature, it is easily affected by external forces to produce cracks, and lithium metal can easily grow along the pores and cracks of the electrolyte layer, thereby causing short circuit problems. Through a lot of research, the inventors of this application proposed to reduce the porosity of the solid electrolyte membrane (such as less than 15%) and increase the hardness of the solid electrolyte membrane (such as more than 0.2GPa) to achieve the purpose of inhibiting the growth of lithium dendrites along the pores and cracks in the solid electrolyte layer, so that the lithium metal negative electrode is not easy to short-circuit in the all-solid-state battery. See below for a description of the specific technical solution.

[0042] In a first aspect, in some embodiments, a solid electrolyte membrane is provided, the solid electrolyte membrane comprising a first solid electrolyte layer and a second solid electrolyte layer disposed on the surface of the first solid electrolyte layer. The first solid electrolyte layer comprises a first solid electrolyte; the second solid electrolyte layer comprises a second solid electrolyte, a lithium-philic material and a negative electrode active material, the lithium-philic material is selected from a material suitable for alloying with lithium metal to form a lithium alloy, and the negative electrode active material comprises lithium titanate and / or a carbon material.

[0043] In the present application, the lithiophilic material can alloy with lithium metal, and optionally, the lithiophilic material can be a metal or a non-metallic material. The negative electrode active material can be selected from lithium titanate, or can be selected from a carbon material, or can be selected from a mixed material of lithium titanate and carbon material.

[0044] The solid electrolyte membrane provided by the present invention has a double-layer structure, that is, the solid electrolyte membrane comprises a stacked double-layer structure, the double-layer structure of the double-layer composite solid electrolyte membrane comprises a first solid electrolyte layer and a second solid electrolyte layer, and the second solid electrolyte layer can be arranged on one of the surfaces of the first solid electrolyte layer along the thickness direction.

[0045] The solid electrolyte membrane provided by the embodiment of the present invention can be applied in solid-state batteries, further in all-solid-state batteries, and further in all-solid-state lithium metal batteries.

[0046] When the solid electrolyte membrane of the present invention is applied to a solid-state battery, the first solid electrolyte layer may be disposed close to the positive electrode, and the second solid electrolyte layer may be disposed close to the negative electrode.

[0047] In some preferred embodiments, the lithiophilic material in the second solid electrolyte layer has a relatively high lithium insertion potential, and as an example, the lithium insertion potential of the lithiophilic material is ≥ 0.3 V. Thus, by adding a lithiophilic material having a lithium insertion potential of 0.3 V or more, the phenomenon of lithium metal precipitating between the first solid electrolyte layer and the second solid electrolyte layer and causing a short circuit can be effectively prevented.

[0048] In some preferred embodiments, the lithium-philic material in the second solid electrolyte layer has a high volume expansion rate after alloying. As an example, the volume expansion rate of the lithium-philic material after alloying with lithium metal to form a lithium alloy is ≥50%. Therefore, the volume expansion rate of the lithium-philic material after alloying with lithium metal is above 50%, and they contact and fuse with each other to form a high-density alloy layer with extremely low porosity, and the hardness can reach about 1GPa or more, so that based on its low porosity and high hardness, it can remain intact during the cycle, is not easily penetrated by lithium dendrites, and can also resist the destructiveness caused by uneven stress distribution of the battery to a certain extent.

[0049] It should be pointed out that the lithium insertion potential of the above-mentioned lithiophilic material can be 0.3V, 0.35V, 0.4V, 0.45V or above 0.45V, and the present application does not limit the upper limit of the lithium insertion potential of the lithiophilic material; the volume expansion rate of the above-mentioned lithiophilic material after alloying can be 50%, 55%, 60%, 65%, 70% or above 70%, and the present application does not limit the specific numerical value of the volume expansion rate.

[0050] It should be understood that the technical problem solved by the present application is mainly to achieve the purpose of inhibiting the production of lithium dendrites by designing the structure and composition of the all-solid electrolyte membrane with a multilayer structure. To achieve this purpose, the porosity of the solid electrolyte membrane is reduced (such as below 15%) and the hardness of the solid electrolyte membrane is increased (such as 0.2 GPa or above), so as to inhibit the growth of lithium dendrites along the pores and cracks in the solid electrolyte layer, so that the lithium metal negative electrode is not easy to short-circuit in the all-solid-state battery.

[0051] The provided all-solid electrolyte membrane with a multilayer structure has a higher compaction density and a higher hardness. It utilizes a high proportion of lithium-affinity materials (such as metals and non-metallic materials) with a high lithium insertion potential and capable of alloying with lithium metal. The volume expansion caused by alloying greatly improves the density and hardness of the electrolyte layer on the side in contact with the lithium metal, thereby preventing the penetration of lithium dendrites. The alloy also has a high ionic conductivity. By superimposing and doping components with a high ionic conductivity and good affinity for lithium (such as negative electrode active materials), the ionic conductivity of the electrolyte layer can reach about 10 - 3 mS / cm or above, which meets actual needs and makes it possible to prepare all-solid-state lithium metal batteries with high rate and long-term stable cycle.

[0052] In the present application, the first solid electrolyte layer in the solid electrolyte membrane with a multilayer structure is located on the positive electrode side, which can conduct active ions such as lithium ions while isolating electronic conduction. The second solid electrolyte layer is located on the negative electrode side, which can inhibit the growth of lithium dendrites. The principle of the solid electrolyte membrane in the present application to inhibit the growth of lithium dendrites is as follows:

[0053] By setting a lithium-philic material (such as metal and non-metallic material) with a high lithium insertion potential that can be alloyed in the second solid electrolyte layer, the lithium-philic material and lithium metal are alloyed to expand and then fuse with each other to compress the pores, so that the second solid electrolyte layer is almost free of pores. At the same time, the high hardness makes it difficult to crack, so that lithium dendrites can neither grow along the pores of the electrolyte nor pierce the second solid electrolyte layer, so that lithium metal can work stably; in addition, the high lithium insertion potential ensures that even if the second solid electrolyte layer has a high electronic conductivity after alloying, lithium metal will not precipitate between the first solid electrolyte layer and the second solid electrolyte layer. In this way, the growth of lithium dendrites can be inhibited.

[0054] In addition, the addition of negative electrode active materials such as lithium titanate, carbon materials and the like in the second solid electrolyte layer can induce uniform deposition of lithium ions and improve the physical contact between lithium metal and the second solid electrolyte layer, which is of positive significance for improving performance.

[0055] Further, in some preferred embodiments, the second solid electrolyte includes a solid electrolyte having a first particle size and a solid electrolyte having a second particle size, wherein the first particle size and the second particle size are different, that is, the second solid electrolyte includes a solid electrolyte with mixed large and small particles. By selecting and setting a solid electrolyte with a combination of large and small particles, the transmission distance of lithium ions in the second solid electrolyte layer can be effectively reduced, so that a lower electrolyte ratio can also enable the second solid electrolyte layer to have sufficient lithium ion conductivity.

[0056] It should be pointed out that the present application does not limit the specific range of the first particle size and the second particle size. As long as it contains solid electrolytes of different particle sizes, those skilled in the art can choose to set it according to actual conditions. For example, the first particle size can be 0.1μm to 2μm, and the second particle size can be 2μm to 10μm. In the present application, the above-mentioned first particle size, i.e., the small particle size electrolyte, can play a role in full contact with other substances, and a small amount of the second particle size, i.e., large particles, can act as a lithium transmission bridge, which can reduce the ion transmission distance and improve ion conductivity.

[0057] Thus, based on the above settings, the solid electrolyte membrane of the present application can effectively inhibit the growth of lithium dendrites, and then the solid-state battery using the solid electrolyte membrane provided by the present application can effectively inhibit the growth of lithium metal dendrites, so that solid-state batteries such as all-solid-state lithium metal batteries can achieve long cycles without short circuits; the present application improves the deposition uniformity of lithium metal, which can make the performance of solid-state batteries more stable during the cycle process. The solid electrolyte membrane of the present application can also improve the rate performance of all-solid-state lithium metal batteries. After long-term use, the alloying material in the second solid electrolyte layer in the solid electrolyte membrane of the present application can also participate in charging and discharging after the negative electrode lithium metal is consumed, which is beneficial to further improve the working life of the battery. In addition, the solid electrolyte membrane of the present application is easier to implement in terms of technology, such as being directly implemented through existing electrolyte membrane preparation processes.

[0058] In some embodiments, the first solid electrolyte includes any one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte, or lithium nitride, or a combination of at least two thereof.

[0059] As an example, the first solid electrolyte may be selected from LPSC, Li 2 SP 2 S 5 , LGPS, LLZO, LATP, halides, lithium nitride (Li 3 N) and the like. For the sake of brevity, the combinations within the above range are not listed one by one.

[0060] By including the first solid electrolyte in the first solid electrolyte layer, it can mainly play the role of conducting lithium ions while isolating electron conduction.

[0061] In some embodiments, the second solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte, or lithium nitride.

[0062] As an example, the second solid electrolyte may be selected from LPSC, Li 2 SP 2 S 5 , LGPS, LLZO, LATP, halides, lithium nitride (Li 3 N) and the like. For the sake of brevity, the combinations within the above range are not listed one by one.

[0063] By including the second solid electrolyte in the second solid electrolyte layer, it is possible to mainly play a role in reducing the interface resistance with the first solid electrolyte layer.

[0064] In the present application, the first solid electrolyte and the second solid electrolyte may be of the same type, or may be of different types, without limitation.

[0065] In addition, the present application is not limited to these first solid electrolytes and second solid electrolytes. The present application can also use other known materials that can be used as solid electrolytes for solid-state batteries.

[0066] In the present application, the second solid electrolyte layer mainly includes a second solid electrolyte, a lithium-philic material and a negative electrode active material, wherein the lithium-philic material can be selected from metals or non-metallic materials that can be alloyed and have a high lithium insertion potential, and can play a role in inhibiting lithium dendrites. In some embodiments, the lithium-philic material includes Si (silicon), SiO x Any one or a combination of at least two of Si (silicon oxide), SiC (silicon carbide), Ge (germanium), Sn (tin), Al (aluminum), In (indium), Mg (magnesium), Sb (antimony), Zr (zirconium), Mn (manganese), Ce (cerium), Y (yttrium), La (lanthanum) or Sc (scandium). For the sake of brevity, the combinations within the above range are not listed one by one. Wherein, x ≥ 0.5.

[0067] The above-mentioned several lithiophilic materials can be alloyed with lithium metal, and have a high lithium insertion potential. By using a lithiophilic material with a lithium insertion potential of more than 0.3V, lithium metal can be effectively prevented from precipitating between the first solid electrolyte layer and the second solid electrolyte layer to cause a short circuit. In addition, the volume expansion rate of the above-mentioned several lithiophilic materials after alloying with lithium metal is more than 50%. They contact and fuse with each other to form a highly dense alloy layer with extremely low porosity, and the hardness can reach more than about 1GPa. Therefore, based on its low porosity and high hardness, it can remain intact during the cycle, is not easily penetrated by lithium dendrites, and can also resist the destructiveness caused by uneven stress distribution of the battery to a certain extent.

[0068] In some embodiments, the average particle size of the lithiophilic material is 0.01 μm to 100 μm. Preferably, the average particle size of the lithiophilic material is 0.01 μm to 10 μm. More preferably, the average particle size of the lithiophilic material is 0.01 μm to 2 μm. As an example, the average particle size of the lithiophilic material can be 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 4 μm, 5 μm, 8 μm, 10 μm, 20 μm, 40 μm, 50 μm, 80 μm, 100 μm, or a range consisting of any two of the above values.

[0069] By controlling the particle size of the lithiophilic material within the above range, the lithiophilic material can be better filled in the gaps between the solid electrolyte particles without affecting the continuous contact between the solid electrolyte particles, thereby reducing or avoiding the impact on the ion conduction and conductivity of the electrolyte.

[0070] In the present application, the negative electrode active material in the second solid electrolyte layer may be selected from lithium titanate and / or carbon material, wherein, in some embodiments, the carbon material includes at least one of graphite, hard carbon or soft carbon. That is, the above-mentioned negative electrode active material may be selected from any one or a combination of at least two of lithium titanate, graphite, hard carbon or soft carbon. For the sake of brevity, the combinations within the above range are not listed one by one.

[0071] The present application improves the affinity between the second solid electrolyte layer and lithium metal by adding the above-mentioned several negative electrode active materials to the second solid electrolyte layer, improves the physical contact between lithium metal and the second solid electrolyte layer, and further induces the uniform deposition of lithium ions on the negative electrode side. It should be understood that the selected several negative electrode active materials have a certain affinity for lithium, which has a positive effect on improving the performance of the solid electrolyte membrane.

[0072] Thus, in the second solid electrolyte layer, the second solid electrolyte, the lithium-philic material and the negative electrode active material are arranged in a coordinated manner, and a higher ionic conductivity is shown during operation, so that the overall ionic conductivity of the second solid electrolyte layer can reach 10 -3 mS / cm or above, effectively improving the ionic conductivity.

[0073] In some embodiments, the mass ratio of the second solid electrolyte, the lithiophilic material, and the negative electrode active material is (10-50): (50-80): (10-20). As an example, the mass ratio of the second solid electrolyte, the lithiophilic material, and the negative electrode active material can be any one of 10:80:10, 15:70:15, 25:65:10, 30:60:10, 20:70:10, or a range between any two of them.

[0074] By controlling the mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material within the above range, it helps to avoid the phenomenon of excessive porosity of the second solid electrolyte layer after molding due to excessive content of the second solid electrolyte. It also helps to ensure that the content of the lithium-philic material and the negative electrode active material is within an appropriate range, effectively inhibiting the growth of lithium dendrites, while avoiding affecting the electrical properties of the solid electrolyte, thereby reducing the risk of short circuit between the positive and negative electrodes and improving battery safety.

[0075] In some embodiments, the first solid electrolyte layer further includes a first binder, that is, the first solid electrolyte layer is mainly composed of a first solid electrolyte and a first binder. The mass fraction of the first binder in the first solid electrolyte layer is 2% to 10%. Preferably, the mass fraction of the first binder in the first solid electrolyte layer is 4% to 6%. As an example, the mass fraction of the first binder in the first solid electrolyte layer can be any one of 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range value between any two of them.

[0076] In some embodiments, the second solid electrolyte layer further includes a second binder, that is, the second solid electrolyte layer is mainly composed of a second solid electrolyte, a lithium-philic material, a negative electrode active material, and a second binder. The mass fraction of the second binder in the second solid electrolyte layer is 2% to 10%. Preferably, the mass fraction of the second binder in the second solid electrolyte layer is 4% to 6%. As an example, the mass fraction of the second binder in the second solid electrolyte layer can be any one of 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range value between any two of them.

[0077] In the present application, in order to improve the adhesion between the first solid electrolyte layer and the second solid electrolyte layer and improve the bonding force between the two, a first binder and a second binder are respectively added to the first solid electrolyte layer and the second solid electrolyte layer. The first binder and the second binder can be conventional binders used in batteries.

[0078] As an example, the first binder may be selected from one or more binders such as styrene-butadiene rubber, nitrile rubber, ethyl cellulose, polyvinylidene fluoride, and polyacrylate.

[0079] As an example, the second binder may be selected from one or more binders such as styrene-butadiene rubber, nitrile rubber, ethyl cellulose, polyvinylidene fluoride, polyacrylate, and the like.

[0080] In the present application, the first binder and the second binder may be of the same type, or may be of different types, without limitation. In addition, in other embodiments, any binder known in the art that can be used in batteries may also be used, which will not be listed here one by one.

[0081] In some embodiments, the thickness of the first solid electrolyte layer is 5 μm to 100 μm. Preferably, the thickness of the first solid electrolyte layer is 10 μm to 30 μm. As an example, the thickness of the first solid electrolyte layer can be 5 μm, 8 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, or a range consisting of any two of the above values.

[0082] By adjusting the thickness of the first solid electrolyte layer within the above range, it is more convenient to integrate the electrolyte membrane into the battery cell, and the thickness can be reduced as much as possible under the premise of complete membrane formation to improve the overall energy density of the battery. If the thickness is too thin, the mechanical properties of the electrolyte membrane will be reduced.

[0083] In some embodiments, the thickness of the second solid electrolyte layer is 5 μm to 100 μm. Preferably, the thickness of the second solid electrolyte layer is 5 μm to 20 μm. As an example, the thickness of the second solid electrolyte layer can be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, or a range consisting of any two of the above values.

[0084] By adjusting the thickness of the second solid electrolyte layer within the above range, the thickness can be reduced as much as possible under the premise of complete film formation to improve the overall energy density of the battery; in addition, it is also beneficial to improve the effect of the solid electrolyte membrane in inhibiting the growth of lithium dendrites.

[0085] In a second aspect, in some embodiments, a method for preparing the solid electrolyte membrane according to the first aspect is provided, the method comprising:

[0086] preparing a first solid electrolyte layer; and

[0087] forming a second solid electrolyte layer on the first solid electrolyte layer;

[0088] The method for preparing the first solid electrolyte layer comprises: mixing the first solid electrolyte, the first binder and the first solvent, and then homogenizing, coating and drying;

[0089] The method of forming the second solid electrolyte layer includes: mixing the second solid electrolyte, the lithium-philic material, the negative electrode active material, the second binder and the second solvent, followed by slurrying, coating and drying.

[0090] It should be understood that the “method for preparing a solid electrolyte membrane” and the aforementioned “solid electrolyte membrane” are based on the same inventive concept, and all the features and advantages described above for the “solid electrolyte membrane” are also applicable to the “method for preparing a solid electrolyte membrane” and will not be elaborated here one by one.

[0091] In the present application, the first solid electrolyte layer can be prepared first, such as by wet coating, and then the second solid electrolyte layer can be prepared by wet coating, and then the first solid electrolyte layer and the second solid electrolyte layer are compounded to obtain a double-layer solid electrolyte membrane. The preparation method of the solid electrolyte membrane is simple in process, easy to operate, and has strong feasibility. It is easy to implement in process, such as by using existing electrolyte membrane preparation process equipment, and the prepared solid electrolyte membrane has excellent performance and low cost, and is easy to realize industrial production.

[0092] In some specific embodiments, the method for preparing the solid electrolyte membrane comprises the following steps (a) and (b):

[0093] Step (a), preparing the first solid electrolyte layer by wet coating, comprising:

[0094] The first binder is dissolved in the first solvent, the first solid electrolyte is weighed according to the calculated solid content and added to the first solvent, the first binder, the first solid electrolyte and the first solvent are fully mixed to obtain a first slurry; then, the first slurry is coated on the molded substrate, and after drying, a first solid electrolyte layer can be obtained.

[0095] Optionally, the above-mentioned forming substrate can be aluminum foil, release film, etc. It should be understood that the aluminum foil, release film, etc. as the forming substrate will be removed after the solid electrolyte membrane is transferred to the negative electrode during the battery preparation stage.

[0096] Optionally, the mass fraction of the first binder in the first solid electrolyte layer is 2% to 10%, preferably 4% to 6%.

[0097] Optionally, the solid content in the first slurry is 30% to 70%, preferably 40% to 50%.

[0098] Optionally, the first solvent may be selected from one or more non-polar solvents such as toluene, xylene, ethyl acetate, butyl acetate, butyl butyrate, anisole, etc.

[0099] Step (b), preparing the second solid electrolyte layer by wet coating, and compounding the second solid electrolyte layer with the first solid electrolyte layer, specifically comprises:

[0100] Dry-mixing and grinding the component materials such as the second solid electrolyte, the lithium-philic material and the negative electrode active material according to proportion;

[0101] The second binder is dissolved in the second solvent, the second solid electrolyte, the lithium-philic material and the negative electrode active material are weighed according to the calculated solid content and added to the second solvent, the second binder, the second solid electrolyte, the lithium-philic material, the negative electrode active material and the second solvent are fully mixed to obtain a second slurry; then, the second slurry is coated on the surface of the first solid electrolyte layer, and after drying, a solid electrolyte membrane with a double-layer structure can be obtained.

[0102] Optionally, the mass fraction of the second binder in the second solid electrolyte layer is 2% to 10%, preferably 4% to 6%.

[0103] Optionally, the mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is (10-50): (50-80): (10-20).

[0104] Optionally, the solid content in the second slurry is 30% to 70%, preferably 40% to 50%.

[0105] Optionally, the second solvent may be selected from one or more non-polar solvents such as toluene, xylene, ethyl acetate, butyl acetate, butyl butyrate, anisole, etc.

[0106] It should be understood that the first solvent and the second solvent may be of the same type or of different types, and this is not limited. In addition, in other embodiments, other non-polar solvents known in the art that can be used in batteries may also be used, which are not listed here one by one.

[0107] In the present application, the prepared solid electrolyte membrane can be subsequently transferred to the negative electrode sheet (such as a lithium metal negative electrode) by transfer. After the transfer, the molding substrate (aluminum foil, release film, etc.) can be removed. The second solid electrolyte layer is in contact with the negative electrode side, and the first solid electrolyte layer is located away from the negative electrode side. The positive electrode (such as a high-nickel ternary positive electrode) is attached to one side of the first solid electrolyte layer, encapsulated, and pressurized (about 500Mpa) in an isostatic pressing device for one-piece molding to prepare an all-solid-state soft-pack battery.

[0108] In a third aspect, in some embodiments, a battery is provided, which includes a positive electrode, a negative electrode and a solid-state electrolyte membrane or a solid-state electrolyte membrane prepared according to the aforementioned method; wherein the solid-state electrolyte membrane is arranged between the positive electrode and the negative electrode, the positive electrode is arranged close to the first solid-state electrolyte layer, and the negative electrode is arranged close to the second solid-state electrolyte layer.

[0109] Optionally, the battery can be an all-solid-state lithium metal battery.

[0110] Optionally, the negative electrode may be a lithium metal negative electrode. Optionally, the thickness of the lithium metal negative electrode is 20 μm to 50 μm.

[0111] It should be noted that in this embodiment, the specific materials and structures of the positive electrode current collector and the positive electrode active material layer in the positive electrode are not limited, and the positive electrode structure and components that are well known in the art and can be used for secondary batteries can be selected.

[0112] Since the battery provided in the embodiment of the present invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0113] In order to better understand the present invention, the specific implementation process of the present invention will be described in detail below in a specific implementation mode. The implementation methods described below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application. If no specific technology or conditions are specified in the implementation method, the technology or conditions described in the literature in the field or the product specification shall be followed.

[0114] Example 1

[0115] 1. Preparation of solid electrolyte membrane, including the following steps:

[0116] The first solid electrolyte layer and the second solid electrolyte layer are prepared by a wet method, comprising:

[0117] The first binder styrene-butadiene rubber (SBR) is dissolved in xylene, the sulfide solid electrolyte LPSC is added to the xylene, and the SBR, LPSC and xylene are fully and evenly mixed, wherein the mass ratio of LPSC to SBR is 95:5, to obtain a first slurry with a solid content of 50%; then, the first slurry is coated on the surface of the molded substrate release film, and after drying, a first solid electrolyte layer can be obtained.

[0118] The sulfide solid electrolyte LPSC, the lithium-philic material single silicon Si (lithium insertion potential 0.5-0.6V, particle size 1μm) and the negative electrode active material hard carbon are dry-mixed in a ratio of 25:60:15, and fully ground for more than 1 hour to obtain a uniformly mixed mixed material; the mixed material and the second binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 95:5, and the mixed material, SBR and xylene are fully mixed to obtain a second slurry with a solid content of 50%; then, the second slurry is coated on the surface of the above-mentioned first solid electrolyte layer, and after drying, a solid electrolyte membrane with a double-layer structure can be obtained.

[0119] 2. Preparation of solid-state batteries, including the following steps:

[0120] A lithium metal negative electrode is used as the negative electrode, and the thickness of the lithium metal negative electrode is 30 μm.

[0121] The preparation of the positive electrode includes: dissolving the binder styrene butadiene rubber (SBR) in a non-polar solvent (xylene) and fully dissolving it to obtain a mixed solution; dry-mixing the positive electrode active material ternary material NCM, the sulfide electrolyte LPSC, and the conductive agent vapor-grown carbon fiber (VGCF), and fully grinding it for more than 1 hour to obtain a uniformly mixed mixed material; adding the above mixed material to the above mixed solution to obtain a slurry with a solid content of 40-60% (the mass ratio of the binder, the positive electrode active material, the sulfide electrolyte LPSC and the conductive agent VGCF is 1:79:19:1), uniformly coating the slurry on an aluminum foil current collector, and baking to obtain a composite positive electrode sheet. The surface capacity of the positive electrode is 5mAh / cm 2 .

[0122] The second solid electrolyte layer in the prepared double-layer solid electrolyte membrane is laminated to the lithium metal negative electrode, and then rolled. The distance between the rollers is adjusted so that the solid electrolyte membrane can be completely transferred to the surface of the lithium metal negative electrode, cut into pieces, and then the composite positive electrode is cut into a uniform or slightly smaller area, and attached to the side of the first solid electrolyte layer in the solid electrolyte membrane, packaged, and isostatically pressed (500Mpa) to obtain an all-solid-state lithium metal battery.

[0123] The resulting lithium metal battery was tested in the voltage range of 2.5-4.3V.

[0124] Example 2

[0125] The difference between Example 2 and Example 1 is that:

[0126] In the first solid electrolyte layer, the mass ratio of LPSC to SBR is 97:3;

[0127] In the second solid electrolyte layer, the mass ratio of the mixed material to SBR is 97:3.

[0128] The rest are the same as in Example 1.

[0129] Example 3

[0130] The difference between Example 3 and Example 1 is that:

[0131] In the first solid electrolyte layer, the mass ratio of LPSC to SBR is 92:8;

[0132] In the second solid electrolyte layer, the mass ratio of the mixed material to SBR is 92:8.

[0133] The rest are the same as in Example 1.

[0134] Example 4

[0135] The difference between Example 4 and Example 1 is that:

[0136] The mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is 10:80:10.

[0137] The rest are the same as in Example 1.

[0138] Example 5

[0139] The difference between Example 5 and Example 1 is that:

[0140] The mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is 30:50:20.

[0141] The rest are the same as in Example 1.

[0142] Example 6

[0143] The difference between Example 6 and Example 1 is that:

[0144] The mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is 65:20:15.

[0145] The rest are the same as in Example 1.

[0146] Example 7

[0147] The difference between Example 7 and Example 1 is that:

[0148] The particle size of Si, a single substance of the lithiophilic material, is 7 μm.

[0149] The rest are the same as in Example 1.

[0150] Example 8

[0151] The difference between Example 8 and Example 1 is that:

[0152] The lithiophilic material used is Sn (lithium insertion potential 0.4 V, particle size 1 μm).

[0153] The rest are the same as in Example 1.

[0154] Example 9

[0155] The difference between Example 9 and Example 1 is that:

[0156] The negative electrode active material is lithium titanate.

[0157] The rest are the same as in Example 1.

[0158] Example 10

[0159] The difference between Example 10 and Example 1 is that:

[0160] In the second solid electrolyte layer, sulfide solid electrolyte LPSC (small particle size 0.1-2 μm), sulfide solid electrolyte LPSC (large particle size 2-10 μm), Si and hard carbon are dry-mixed in a ratio of 20:5:60:15.

[0161] The rest are the same as in Example 1.

[0162] Comparative Example 1

[0163] The main difference between Comparative Example 1 and Example 1 is:

[0164] The solid electrolyte membrane of Comparative Example 1 omits the second solid electrolyte layer, that is, the solid electrolyte membrane of Comparative Example 1 only contains the first solid electrolyte layer.

[0165] The rest are the same as in Example 1.

[0166] Comparative Example 2

[0167] The main difference between Comparative Example 2 and Example 1 is:

[0168] In the second solid electrolyte layer of the solid electrolyte membrane of Comparative Example 2, the lithium-philic material is omitted, and in the second solid electrolyte layer, the mass ratio of the second solid electrolyte to the negative electrode active material is 30:70.

[0169] The rest are the same as in Example 1.

[0170] Comparative Example 3

[0171] The main difference between Comparative Example 3 and Example 1 is:

[0172] In the second solid electrolyte layer of the solid electrolyte membrane of Comparative Example 3, the negative electrode active material is omitted, and in the second solid electrolyte layer, the mass ratio of the second solid electrolyte to the lithium-philic material is 70:30.

[0173] The rest are the same as in Example 1.

[0174] Comparative Example 4

[0175] The main difference between Comparative Example 4 and Example 1 is:

[0176] In the second solid electrolyte layer of the solid electrolyte membrane of Comparative Example 4, the second solid electrolyte and the negative electrode active material are omitted, and in the second solid electrolyte layer, the lithium-philic material accounts for 100% of the mixed material.

[0177] The rest are the same as in Example 1.

[0178] Performance Testing

[0179] The solid electrolyte membranes and solid-state batteries obtained in the above-mentioned embodiments and comparative examples were subjected to performance tests.

[0180] 1. Porosity test: The porosity test was performed using FIM-SEM. The batteries before and after pressure molding in each embodiment and comparative example were disassembled, and the battery cross-sections were longitudinally cut to obtain the positions of the first solid electrolyte layer and the second solid electrolyte layer under SEM. The FIB layer-by-layer cutting and SEM imaging were performed alternately under software control. Finally, three-dimensional reconstruction was performed by software and the porosity of the first solid electrolyte layer and the second solid electrolyte layer was calculated, and the data was recorded.

[0181] 2. The batteries prepared in the above embodiments and comparative examples were subjected to charge and discharge tests, with the charge and discharge voltage range set at 2.5-4.3V.

[0182] (1) First coulombic efficiency (first efficiency) test: Within the above voltage range (2.5-4.3V), charge and discharge for one cycle at a constant current of 0.1C (charge at a constant current of 0.1C to 4.3V, and then discharge at a constant current of 0.1C to 2.5V for one cycle), and observe whether a short circuit occurs. The result of (0.1C discharge capacity / 0.1C charge capacity*100%) is used as an indicator for evaluating the first efficiency of the battery. A short-circuited battery means that it cannot pass the first efficiency test and is recorded as "-", with a note of first charge short circuit.

[0183] (2) Rate performance test: Carry out 0.1C, 0.2C, 0.3C, 0.5C and 1C constant current charge and discharge tests in the above voltage range (2.5-4.3V) in sequence to observe whether the battery will short-circuit at different rates. The ratio of (1C discharge capacity / 0.1C discharge capacity*100%) is used as an indicator to evaluate the battery rate performance. A short-circuited battery means that it cannot pass the rate test and is recorded as "-". The rate value when the short circuit occurs is recorded as a note.

[0184] (3) Cycle performance test: Within the above voltage range (2.5-4.3V), set the current of 0.2C for constant current charge and discharge, and observe whether the battery will short-circuit during the cycle charge and discharge process. The result of (100th cycle discharge capacity / 1st cycle discharge capacity*100%) is used as an indicator to evaluate the battery cycle performance. A short-circuited battery means that it cannot pass the cycle test and is recorded as "-". The number of cycles when the short circuit occurs is noted.

[0185] The test results are shown in Table 1 below.

[0186] Table 1

[0187]

[0188] Note: In Table 1, before molding refers to the battery before molding, and after molding refers to the use of isostatic pressing to apply 500mPa pressure to mold the all-solid-state battery, which can then be charged and discharged.

[0189] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-4, the solid-state batteries using the solid electrolyte membranes prepared in Examples 1-10 of the present invention have first coulombic efficiency, rate performance and capacity retention rate during the charge and discharge process, which improves the cycle life of the battery, reduces the risk of short circuit in the battery, and improves the safety of the battery.

[0190] Among them, through the analysis and comparison of Examples 1-3, it can be seen that adjusting the ratio of the binder to the solid electrolyte and other substances in the solid electrolyte layer has a certain influence on the obtained solid electrolyte membrane. In general, the lithium metal battery obtained by the solid electrolyte membrane of Example 1 shows good comprehensive performance; while Example 2 reduces the content of the binder, which can slightly improve the rate performance, but the integrity of the electrolyte membrane is slightly reduced, affecting the stability of the cycle; Example 3 increases the content of the binder, and the electrolyte membrane is relatively smooth, but affects the rate performance. Therefore, by making the content of the binder within an appropriate range, the rate performance and cycle stability of the battery can be guaranteed.

[0191] Through the analysis and comparison of Example 1 and Examples 4-6, it can be seen that adjusting the ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material in the second solid electrolyte layer has a certain effect on the obtained solid electrolyte membrane. The proportion of lithium-philic materials in Example 4 is relatively high, that is, the proportion of expansive materials increases, and the battery runs smoothly at a lower current density, but a short circuit will occur at a large current (0.5C). Studies have found that this is mainly due to the insufficient ion conductivity of the second solid electrolyte layer. The proportion of lithium-philic materials in Example 5 decreases slightly, that is, the proportion of expansive materials decreases to 50%, and the battery can operate more stably, but long cycles are still subject to certain challenges. The proportion of lithium-philic materials in Example 6 decreases more, that is, the proportion of expansive materials decreases to 20%, and the second solid electrolyte layer has difficulty in inhibiting the growth of lithium dendrites, and short circuits occur in short cycles. Therefore, it is necessary to make the ratio of the two solid electrolytes, the lithium-philic material and the negative electrode active material in the second solid electrolyte layer within an appropriate range to ensure the content of the added lithium-philic material, which can effectively inhibit the growth of lithium dendrites, reduce the occurrence of short circuits, and improve the safety of the battery.

[0192] Through the analysis and comparison of Example 1 and Example 7, it can be known that adjusting the particle size of the lithiophilic material, such as increasing the particle size of the lithiophilic material, can slightly increase the porosity of the solid electrolyte membrane after molding, but has little effect on the cycle performance, safety performance, etc. of the battery. Within the appropriate particle size range of the lithiophilic material, the cycle performance, safety performance, etc. of the battery are guaranteed.

[0193] Through the analysis and comparison of Example 1 and Example 8, it can be seen that the performances exhibited by the several lithium-philic materials provided by the present invention are not much different, and all of them can make the prepared solid electrolyte membrane show good first coulomb efficiency, rate performance and capacity retention rate, and also reduce the risk of short circuit of the battery, and improve the safety of the battery. Through the analysis and comparison of Example 1 and Example 9, it can be seen that compared with the hard carbon negative electrode active material, the solid-state battery of the solid electrolyte membrane made of lithium titanate negative electrode active material can operate stably. Although the first coulomb efficiency and cycle performance are slightly reduced, compared with the existing comparative example, the use of several negative electrode active materials provided by the present invention can make the prepared solid electrolyte membrane show good first coulomb efficiency, rate performance and capacity retention rate, and improve the safety of the battery.

[0194] Through the analysis and comparison of Example 1 and Example 10, it can be seen that by using second solid electrolytes with different particle sizes in combination, the second solid electrolyte layer can have sufficient lithium ion conductivity, thereby improving the rate performance of the battery.

[0195] Through the analysis and comparison of Example 1 and Comparative Example 1, it can be seen that the solid electrolyte membrane omitting the second solid electrolyte layer cannot effectively inhibit the growth of lithium dendrites, and a short circuit occurs during the first 0.1C charge of the full battery, which reduces the safety of the battery.

[0196] Through the analysis and comparison of Example 1 and Comparative Example 2, it can be seen that by omitting the lithium-philic material in the second solid electrolyte layer, the growth of lithium dendrites cannot be effectively inhibited, and the battery will short-circuit under large current, and the cycle attenuation will be more serious, indicating that the lithium-philic material has an irreplaceable role in lithium transmission. Through the analysis and comparison of Example 1 and Comparative Example 3, it can be seen that by omitting the negative electrode active material in the second solid electrolyte layer, the battery will short-circuit under large current, and the first effect will decrease, which shows that the negative electrode active material in the second solid electrolyte layer has a positive effect on improving the first effect and safety performance of the battery. Through the analysis and comparison of Example 1 and Comparative Example 4, it can be seen that by omitting the second solid electrolyte and the negative electrode active material in the second solid electrolyte layer, the battery can run smoothly for 60 laps at a small current, but a short circuit will occur at 0.3C, indicating that the lithium-philic material, that is, the expansive material, can also transmit lithium ions after lithium insertion, but the ionic conductivity is low.

[0197] also, Figure 1 The first cycle charge and discharge curve (0.1C) of the solid-state battery of Example 1 of the present invention is shown. Figure 1 It can be seen that during the discharge process, the battery potential is maintained above 3.5V, which is conducive to further improving the battery energy density. It is a typical lithium metal battery curve, indicating that the battery is a lithium metal battery.

[0198] Figure 2 The cycle test data (0.2C) of the solid-state battery of Example 1 of the present invention is shown. Figure 2 It can be seen from the capacity curve of Example 1 at 0.2C cycle that the solid-state battery is stable in 100 cycles and has a high capacity retention rate.

[0199] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0200] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.

[0201] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0202] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0203] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A solid electrolyte membrane, characterized in that: comprising a first solid electrolyte layer and a second solid electrolyte layer disposed on a surface of the first solid electrolyte layer; The first solid electrolyte layer includes a first solid electrolyte, and the first solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte or lithium nitride; The second solid electrolyte layer comprises a second solid electrolyte, a lithium-philic material and a negative electrode active material, wherein the lithium-philic material is selected from materials suitable for alloying with lithium metal to form a lithium alloy, and the lithium-philic material comprises Si, SiO x , at least one of SiC, Ge, Sn, Al, In, Mg, Sb, Zr, Mn, Ce, Y, La or Sc, wherein x ≥ 0.5; The lithium insertion potential of the lithium-philic material is ≥0.3V, and the volume expansion rate of the lithium-philic material after alloying with lithium metal to form a lithium alloy is ≥50%; The second solid electrolyte includes at least one of a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, a halide solid electrolyte or lithium nitride; The negative electrode active material includes lithium titanate and / or carbon material.

2. The solid electrolyte membrane according to claim 1, characterized in that The average particle size of the lithium-philic material is 0.01 μm to 100 μm.

3. The solid electrolyte membrane according to claim 1, characterized in that The carbon material includes at least one of graphite, hard carbon or soft carbon.

4. The solid electrolyte membrane according to claim 1, characterized in that The mass ratio of the second solid electrolyte, the lithium-philic material and the negative electrode active material is (10-50): (50-80): (10-20).

5. The solid electrolyte membrane according to claim 1, characterized in that The first solid electrolyte layer further includes a first binder, and the mass fraction of the first binder in the first solid electrolyte layer is 2% to 10%; And / or, the second solid electrolyte layer further includes a second binder, and the mass fraction of the second binder in the second solid electrolyte layer is 2% to 10%.

6. The solid electrolyte membrane according to any one of claims 1 to 5, characterized in that: The thickness of the first solid electrolyte layer is 5 μm to 100 μm; And / or, the thickness of the second solid electrolyte layer is 5 μm to 100 μm.

7. The method for preparing a solid electrolyte membrane according to any one of claims 1 to 6, characterized in that: The method comprises: preparing a first solid electrolyte layer; and forming a second solid electrolyte layer on the first solid electrolyte layer; The method for preparing the first solid electrolyte layer comprises: mixing the first solid electrolyte, the first binder and the first solvent, and then homogenizing, coating and drying; The method for forming the second solid electrolyte layer comprises: mixing a second solid electrolyte, a lithium-philic material, a negative electrode active material, a second binder and a second solvent, followed by homogenization, coating and drying.

8. A battery, characterized in that: The battery comprises a positive electrode, a negative electrode and a solid electrolyte membrane according to any one of claims 1 to 6 or a solid electrolyte membrane prepared according to the method of claim 7; The solid electrolyte membrane is arranged between the positive electrode and the negative electrode, the positive electrode is arranged close to the first solid electrolyte layer, and the negative electrode is arranged close to the second solid electrolyte layer.