Saw resonator having electrode structure with improved performance
By forming an amorphous layer and a seed layer on the piezoelectric substrate of the SAW resonator, combined with the ohmic contact layer and wiring layer, the problem of insufficient crystallinity of the high-density metal layer is solved, and the crystallinity and orientation of the electrode are improved. Improved etching quality and performance, enhanced equipment reliability and power resistance.
Patent Information
- Application Number
- CN202410241514.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-04
- Publication Date
- 2024-10-01
AI Technical Summary
When forming a high-density first metal layer in an existing SAW resonator, the crystallinity and orientation are insufficient, resulting in uneven etching and residual material residues, affecting performance and reliability.
Form an amorphous layer on the piezoelectric substrate, superimpose a seed layer and a main electrode layer on it, improve the crystallinity and orientation of the main electrode layer through the seed layer, and add an ohmic contact layer and a wiring layer to the IDT electrode. to maintain etching quality.
The electrode crystallinity and orientation of the SAW resonator are improved, the etching quality is improved, the performance and miniaturization capabilities are enhanced, while unwanted spurious wave modes are avoided, and the reliability and power resistance of the equipment are improved.
Smart Images

Figure CN118740100A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a SAW (Surface Acoustic Wave) resonator with an electrode structure that improves performance and a method for manufacturing the same, and more specifically to a SAW resonator and a method for manufacturing the same. When an electrode with a lattice structure different from that of a piezoelectric substrate is stacked on a piezoelectric substrate, the SAW resonator can improve the crystallinity and orientation of the electrode, thereby improving electrical performance. Background Art
[0002] Surface acoustic waves (SAW) are waves that propagate along the surface of elastic solids. The energy of these elastic surface waves is concentrated near the surface and is equivalent to mechanical fluctuations. Surface acoustic wave elements are electromechanical elements that utilize the interaction between surface acoustic waves and semiconductor conductive electrons, and utilize surface acoustic waves that are conducted on the surface of piezoelectric crystals. These surface acoustic wave elements can have a very wide range of applications in industries such as sensors, oscillators, and filters, and can be miniaturized and lightweight, and have many advantages such as robustness, stability, sensitivity, low cost, and real-time performance.
[0003] In line with the production trend of electronic components that require miniaturization, Figure 1 As shown, a structure in which two metals are stacked in an IDT electrode is applied in a SAW resonator.
[0004] Reference Figure 1 , a cross-sectional view of a plurality of IDT electrodes 50 is shown, and a SAW resonator 10 according to the prior art includes a plurality of IDT electrodes 50 which are sequentially stacked on a first metal layer 20 and a second metal layer 30 formed on a substrate 1. The second metal layer 30, as a main electrode layer, may include aluminum (Al) or the like, and the first metal layer 20 may include a metal having a higher density than the second metal layer 30, for example, tungsten (W), platinum (Pt), molybdenum (Mo), copper (Cu) or the like.
[0005] The low-density second metal layer 30 is stacked as a main electrode on the high-density first metal layer 20, so that the acoustic velocity of the surface elastic wave can be reduced, thereby having the effect of contributing to the miniaturization of the resonator 10. However, when the high-density first metal layer 20 is formed by sputtering and the IDT electrode 50 is formed by etching, if the crystallinity and orientation of the formed first metal layer 20 do not reach a certain level, not only the performance cannot be satisfied, but also in the etching process of the first metal layer 20 formed in an amorphous state, the first metal layer 20 is unevenly etched, and the residual material of the first metal layer 20 will remain on the piezoelectric substrate, and an unwanted spurious mode will occur, causing the problem of reduced reliability and power resistance.
[0006]
Prior technical literature
[0007] [Patent Literature]
[0008] (Patent Document 1) Patent Publication No. 10-2003-0057386 Summary of the invention
[0009] The technical problem to be solved by the present invention is to provide a SAW resonator and a method for manufacturing the same, which includes a multi-layered IDT electrode that can improve crystallinity and orientation while maintaining etching quality relative to the miniaturization of a SAW filter and a plurality of metal layers constituting an IDT electrode.
[0010] The technical problems of the present invention are not limited to the technical problems mentioned above, and those skilled in the art can clearly understand other technical problems not mentioned from the following description.
[0011] To solve the above technical problems, a SAW resonator with an electrode structure having improved performance according to some embodiments of the present invention includes: a piezoelectric substrate; and a plurality of IDT electrodes formed on the piezoelectric substrate, the plurality of IDT electrodes respectively including: a seed layer stacked on the surface of the piezoelectric body; and a main electrode layer formed on the seed layer, and an amorphous layer is formed on the upper surface of the piezoelectric layer.
[0012] In some embodiments of the present invention, at least one of the plurality of IDT electrodes is a contact electrode, and the contact electrode may further include an ohmic contact layer formed on the main electrode layer.
[0013] In some embodiments of the present invention, it further includes: a wiring layer, which is formed on the ohmic contact layer and is bonded to the contact electrode, and includes a lower wiring layer, and the ohmic contact layer and the lower wiring layer can form an ohmic contact.
[0014] In some embodiments of the present invention, the ohmic contact layer may include titanium, titanium nitride (TiN), titanium oxide (TiOx), or titanium-tungsten (TiW).
[0015] In some embodiments of the present invention, the main electrode may include a lower main electrode layer and an upper main electrode layer stacked in sequence.
[0016] In some embodiments of the present invention, the lower main electrode layer may include a metal with a higher density than the upper main electrode layer.
[0017] In some embodiments of the present invention, the lower main electrode layer includes at least any one of tungsten (W) or copper (Cu), and the upper main electrode layer may include aluminum (Al).
[0018] In some embodiments of the present invention, the piezoelectric substrate includes: a supporting substrate; an energy confinement layer formed on the supporting substrate; and a piezoelectric layer formed on the energy confinement layer, and the energy confinement layer may include a low-velocity layer and / or a high-velocity layer.
[0019] In some embodiments of the present invention, the seed layer may include at least any one of titanium, titanium nitride (TiN), titanium oxide (TiOx), titanium-tungsten (TiW), and chromium (Cr).
[0020] In some embodiments of the present invention, an insulating layer may be further included between the plurality of IDT electrodes and the amorphous layer.
[0021] In order to solve the above-mentioned technical problems, the manufacturing method of a SAW resonator with an improved electrode structure according to some embodiments of the present invention may include the following steps: preparing a piezoelectric substrate on the surface; performing surface treatment on the surface of the piezoelectric substrate by ion implantation or plasma to form an amorphous layer; forming a seed layer on the amorphous layer; forming a main electrode layer on the seed layer; and etching the seed layer and the main electrode layer to form a plurality of IDT electrodes.
[0022] In some embodiments of the present invention, the step of forming an ohmic contact layer on the main electrode layer may be further included before the step of forming the plurality of IDT electrodes.
[0023] In some embodiments of the present invention, after the step of forming a plurality of IDT electrodes, a step of forming a wiring layer on the ohmic contact layer so as to be coupled to a contact electrode of one of the plurality of IDT electrodes is further included, and the ohmic contact layer and the wiring layer can form an ohmic contact.
[0024] In some embodiments of the present invention, before the step of forming the plurality of IDT electrodes, a step of forming an insulating layer between the seed layer and the amorphous layer may be further included.
[0025] In some embodiments of the present invention, the step of forming the main electrode layer includes the step of sequentially stacking a lower main electrode layer and an upper main electrode layer, and the lower main electrode layer may include a material with a higher density than the upper main electrode layer.
[0026] In some embodiments of the present invention, the lower main electrode layer includes at least any one of tungsten (W) or copper (Cu), and the upper main electrode layer may include aluminum (Al).
[0027] Details of other embodiments are included in the detailed description and drawings.
[0028] According to the SAW resonator with improved electrode structure and the manufacturing method thereof of the embodiment of the present invention, an amorphous layer is formed on the upper surface of the piezoelectric substrate, and the main electrode layer can improve the orientation and crystallinity by lattice alignment through the seed layer formed between the amorphous layer and the main electrode layer. Even in an IDT electrode with a multi-layer structure for miniaturization, the orientation and crystallinity of all the main electrode layers are improved, and the effect of improving the etching quality of the main electrode layer can be obtained through the seed layer. Therefore, it is possible to maintain miniaturization while improving the performance of the SAW resonator.
[0029] In addition, the SAW resonator with an improved electrode structure according to an embodiment of the present invention maintains an ohmic contact state rather than a capacitive contact when an ohmic contact layer is additionally included on an IDT electrode, specifically, on a main electrode layer and then a wiring layer is formed on the IDT electrode.
[0030] Furthermore, when an insulating layer is formed between the piezoelectric substrate having the amorphous layer and the seed layer, the etching quality of the main electrode layer can be further improved without reducing the orientation and crystallinity of the main electrode layer.
[0031] The effects of the present invention are not limited to the effects mentioned above, and those skilled in the art can clearly understand other effects not mentioned from the description of the claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a diagram of a SAW resonator including a plurality of IDT electrodes according to the prior art.
[0033] Figure 2a and Figure 2b is a diagram of a SAW resonator having an enhanced electrode structure according to an embodiment of the present invention.
[0034] Figure 3 It is a diagram for explaining the effect of the SAW resonator according to the embodiment of the present invention.
[0035] Figures 4a to 4c: is a graph for explaining the effect of the SAW resonator according to the embodiment of the present invention.
[0036] Figure 5 is a diagram of a SAW resonator having an enhanced electrode structure according to another embodiment of the present invention.
[0037] Figure 6 is a diagram of a SAW resonator having an improved electrode structure according to yet another embodiment of the present invention.
[0038] Figure 7 is a diagram of a SAW resonator having an enhanced electrode structure according to yet another embodiment of the present invention.
[0039] Figure 8 and Fig. 9 It is used to explain the Figure 6 FIG. 1 is a diagram of the effect of the SAW resonator 300 of the embodiment.
[0040] Fig.10 FIG. 1 is a sequence diagram for explaining a method for manufacturing a SAW resonator having an improved electrode structure according to an embodiment of the present invention.
[0041] Figures 11 to 16 FIG. 1 is a diagram for explaining an intermediate step of a method for manufacturing a SAW resonator having an improved electrode structure according to an embodiment of the present invention.
[0042] Fig.17 FIG. 1 is a sequence diagram for explaining a method for manufacturing a SAW resonator having an improved electrode structure according to another embodiment of the present invention.
[0043] Fig.18 and 19 FIG. 1 is a diagram for explaining an intermediate step of a method for manufacturing a SAW resonator having an improved electrode structure according to another embodiment of the present invention.
[0044] Description of symbols
[0045] 100, 200, 300, 400: SAW resonator 110, 210, 310: substrate
[0046] 111, 211, 311: Support substrate 112, 212, 312: Energy confinement layer
[0047] 113, 213, 313: piezoelectric layer 120, 220, 320: seed layer
[0048] 130, 230, 330: Main electrode layer 150, 250, 350: IDT electrode
[0049] 360: Insulation film
[0050] 470: Ohmic contact layer 480: Wiring layer DETAILED DESCRIPTION
[0051] The advantages, features, and methods of achieving the same of the present invention will become clear when referring to the accompanying drawings and the embodiments described in detail below. However, the present invention is not limited to the embodiments disclosed below, but is implemented in different and diverse forms. This embodiment is only provided to ensure that the disclosure of the present invention is complete and to fully inform the scope of the invention to those with general knowledge in the technical field to which the present invention belongs. The present invention is defined only by the scope of the claims. Throughout the specification, the same reference numerals represent the same constituent elements.
[0052] When a component is “connected to” or “coupled to” another component, it includes the case where it is directly connected or coupled to the other component or where other components are interposed. On the contrary, when a component is “directly connected to” or “directly coupled to” another component, it indicates that there are no other components interposed. “And / or” includes all combinations of each and more than one of the mentioned items.
[0053] The terms used in this specification are intended to illustrate the embodiments, not to limit the present invention. In this specification, the singular also includes the plural, unless otherwise specifically mentioned in a sentence. The use of "comprises" and / or "comprising" in the specification does not exclude the existence or addition of one or more other constituent elements, steps, actions and / or elements in addition to the constituent elements, steps, actions and / or elements mentioned.
[0054] Although the terms first, second, etc. are used to describe various components, these components are not limited by these terms. The purpose of the terms is only to distinguish one component from other components. Therefore, the first component mentioned below can also be the second component within the technical concept of the present invention.
[0055] If there is no other definition, all terms (including technical and scientific terms) used in this specification can be used for the meaning commonly understood by people with general knowledge in the technical field to which the present invention belongs. In addition, the terms defined in the commonly used dictionaries will not be ideally or excessively interpreted unless there is an obvious special definition.
[0056] Figure 2a and 2b is a cross-sectional view of a SAW resonator having an enhanced electrode structure according to an embodiment of the present invention.
[0057] Reference Figure 2a The SAW resonator 100 with an electrode structure having improved performance according to an embodiment of the present invention may include a plurality of IDT electrodes 150 formed on a piezoelectric substrate 110 , including a seed layer 120 and a main electrode layer 130 .
[0058] The piezoelectric substrate 110 may be formed by sequentially stacking an energy confinement layer 112 and a piezoelectric layer 113 on a lower support substrate 111. The support substrate 111 may be formed of, for example, a semiconductor substrate such as silicon, a ceramic substrate, an insulator substrate, or the like.
[0059] The energy confinement layer 112 is a layer that transmits sound at a lower speed or a higher speed than the elastic wave propagated by the piezoelectric layer 113, for example Figure 2b As shown in FIG. 1 , a low-velocity layer 112A is stacked on a high-velocity layer 112B to confine elastic waves to the surface of the high-velocity layer or as shown in FIG. Figure 2a As shown, a high-speed layer or a low-speed layer may also be formed separately. The high-speed layer constituting the energy confinement layer 112 may include at least one of aluminum nitride, aluminum oxide, silicon nitride, silicon oxynitride, silicon, etc., and the low-speed layer may include at least one of a plurality of known materials such as silicon oxide, glass, silicon oxynitride, etc.
[0060] The piezoelectric layer 113 includes a piezoelectric element, may generate an elastic wave from a signal applied to the IDT electrode 150, and may include a substance such as LiTaO3 (LT) and LiNbO3 (LN).
[0061] By performing ion implantation or plasma treatment on the surface of the piezoelectric layer 113, an amorphous layer 114 can be formed on the surface. This is to prevent the film quality of the IDT electrode 150 from being affected by the inherent characteristics such as the lattice structure and angle of the piezoelectric substrate 110. In other words, the amorphous layer 114 is preferably formed on the upper surface of the piezoelectric layer 113 so as not to be too thick in order to invalidate the inherent characteristics of the piezoelectric substrate 110, more specifically, the piezoelectric layer 113.
[0062] exist Figure 2a , etc., show that the amorphous layer 114 formed by performing surface treatment on the piezoelectric layer 113 and the piezoelectric layer 113 at the bottom are completely separated due to the upper and lower relationship, but the present invention is not limited to this. For example, the amorphous layer 114 modified by the surface treatment and the original piezoelectric layer 113 can be mixed and arranged on the top of the piezoelectric substrate 110, and in another embodiment, the amorphous layer 114 can also be formed below the surface of the piezoelectric layer 113.
[0063] A plurality of IDT electrodes 150 may be arranged on the piezoelectric substrate 110. Figure 2aIn the example shown in FIG. 1 , five IDT electrodes 150 are formed on the piezoelectric substrate 110 . However, this is a simplified structure for the purpose of explanation, and it is obvious that more than five IDT electrodes 150 may be arranged to constitute the SAW resonator 100 .
[0064] The IDT electrodes 150 may correspond to a plurality of electrodes alternately extending from two bus bars facing each other on the surface of the piezoelectric substrate 110. The SAW resonator 100 may determine the speed of the surface wave by the interval distance between adjacent IDT electrodes 150, that is, the pitch.
[0065] The IDT electrode 150 may be formed by sequentially stacking a seed layer 120 and a main electrode layer 130 .
[0066] The seed layer 120 may be composed of one of materials having a hexagonal close-packed crystal structure, such as titanium (Ti), magnesium (Mg), zinc (Zn), cadmium (Cd), scandium (Sc), and ruthenium (Ru), or an alloy or a laminated structure of two or more selected from the above materials. Preferably, the above materials may contain a diffusion coefficient of 0.3×10 -6 cm 2 Therefore, the seed layer 120 can be used as a barrier layer to prevent diffusion to the piezoelectric substrate 110 when the main electrode layer 130 is formed.
[0067] In some embodiments of the present invention, the seed layer 120 may be formed to be less than 10 nm. If the seed layer 120 is greater than this value, it helps to reduce etching residues such as the base metal layer 130, but since the titanium and other materials constituting the seed layer 120 also have a large resistance, it will have an adverse effect on the performance of the SAW resonator 100.
[0068] The main electrode layer 130 may be formed on the seed layer 120. The main electrode layer 130 may include, for example, at least one of materials with high conductivity such as copper (Cu), silver (Ag), gold (Au), platinum (Pt), tungsten (W), or an alloy with any of the materials as a main material.
[0069] The main electrode layer 130 forms a lattice alignment structure according to the seed layer 120, thereby improving the crystallinity and orientation during film formation. Figure 3 This is explained in more detail.
[0070] Figure 3 It is a diagram for explaining the effect of the SAW resonator according to the embodiment of the present invention.
[0071] Reference Figure 3, LiTaO3 (LT) contained in the piezoelectric layer 113 and aluminum constituting the main electrode layer 130 have different lattice structures, respectively. In particular, aluminum originally has a cubic structure, and therefore it is difficult to form an alignment structure with LT or LN forming the piezoelectric layer 113. Therefore, as described above, the crystallinity and orientation of the main electrode layer 130 may be reduced, and the etching quality of the main electrode layer 130 may also be reduced.
[0072] However, the SAW resonator 100 according to the embodiment of the present invention may improve orientation and crystallinity through lattice alignment of the main electrode layer 130 formed according to the seed layer 120 formed between the piezoelectric layer 113 and the main electrode layer 130 .
[0073] The degree of miniaturization of the SAW resonator 100 of the present invention is related to the thickness of the main electrode layer 130. In other words, the greater the thickness of the main electrode layer 130, the lower the acoustic velocity of the surface elastic wave caused by the IDT electrode 150 and the lower the period of the IDT electrode 150, thereby miniaturization can be achieved. However, due to the etching quality of the main electrode layer 130, the increase in thickness has been limited, and due to the stacked structure of the IDT electrode 150 included in the SAW resonator 100 of the present invention, the miniaturization of the SAW resonator 100 can be further improved.
[0074] In addition, the piezoelectric layer 113 includes an amorphous layer 114 formed on the surface by ion implantation or plasma treatment, thereby minimizing the influence of the piezoelectric substrate 110, especially minimizing the influence of the inherent lattice structure and angle characteristics of the piezoelectric layer 113, thereby improving the film formation and etching characteristics of the IDT electrode 150.
[0075] Reference Figure 4a , shows the crystallinity graph of the main electrode layer 130 when Ti is inserted into the seed layer 120 (LT / Ti / W / Al graph) and when the seed layer 120 is not inserted (LT / W / Al). As an example of the main electrode layer 130 containing tungsten and aluminum respectively, the horizontal axis is 2Theta and the vertical axis is intensity. The peak value when the seed layer 120 is inserted is much higher, and it can be seen that it is a graph showing the high crystallinity of the main electrode layer 130.
[0076] On the other hand, refer to Figure 4b , a graph showing the orientation of the main electrode layer 130 when Ti is inserted into the seed layer 120 (LT / Ti / W / Al graph) and when the seed layer 120 is not inserted (LT / W / Al). Figure 4bThe XRD intensity in the 111 direction of aluminum of the main electrode layer 140 is shown. As with the previous crystallinity, even if only the peak of the XRD intensity when the seed layer 120 is inserted is considered, it can be seen that the orientation of the base metal layer 130 and the main electrode layer 140 is improved.
[0077] Reference Figure 4c , which shows a graph of the attenuation characteristics of the SAW resonator having the IDT electrode of the present invention in the low frequency band. It can be confirmed that, in the case of the stacked structure having the seed layer 120 and the main electrode layer 130 as in the SAW resonator 100 of the present invention, the performance is equal to or better than that of the case of only forming the main electrode layer 130.
[0078] Figure 5 2 is a diagram of a SAW resonator 200 having an improved electrode structure according to another embodiment of the present invention. It is understood that the components having the same reference numerals as those of the previously described embodiment are the corresponding components, and detailed descriptions thereof are omitted.
[0079] Reference Figure 5 , the main electrode layer 230 of the SAW resonator 200 according to another embodiment of the present invention may be divided into a lower main electrode layer 231 and an upper main electrode layer 232 .
[0080] In order to reduce the speed of the surface acoustic wave transmitted by the IDT electrode 250 , the SAW resonator 200 in the present embodiment may include a main electrode layer 230 structure divided into a lower main electrode layer 231 including a material having a higher density than an upper main electrode layer 232 .
[0081] The lower main electrode layer 231 may include a substance having a higher density than the metal substance constituting the upper main electrode layer 232, such as tungsten (W). For example, the lower main electrode layer 231 and the upper main electrode layer 232 may include tungsten W and aluminum Al, respectively, which are easy to form a hexagonal close-packed crystal structure.
[0082] As described above, by stacking the low-density second metal layer 232 on the high-density lower main electrode layer 231 , the main electrode layer 230 structure can reduce the acoustic velocity of the surface acoustic wave, thereby contributing to miniaturization of the SAW filter 200 .
[0083] In addition, if Figure 3As shown, when the lower main electrode layer 231 and the upper main electrode layer 232 are respectively composed of tungsten and aluminum, tungsten and aluminum have different lattice structures, namely, cubic structures, from LT or LN contained in the piezoelectric layer 213, and therefore it is difficult to form an aligned structure. However, due to the presence of the seed layer 220, the SAW resonator 200 of the present invention can improve orientation and crystallinity by lattice alignment of the metal layers forming the lower main electrode layer 231 and the upper main electrode layer 232.
[0084] Figure 6 is a diagram of a SAW resonator 200 having an enhanced electrode structure according to another embodiment of the present invention.
[0085] Reference Figure 6 According to another embodiment of the present invention, the SAW resonator 300 may include an insulating layer 360 between the IDT electrode 350 and the piezoelectric substrate 310, more specifically, the seed layer 320 and the amorphous layer 314. The insulating layer 360 may include, for example, silicon oxide (SiO2) or silicon nitride (SiN x )wait.
[0086] The insulating layer 360 is formed between the piezoelectric layer 313 and the IDT electrode 350 , so that the etching quality of the IDT electrode 350 can be further improved without reducing the orientation and crystallinity of the main electrode layer 330 .
[0087] When the thickness of the insulating layer 360 becomes too thick, the bandwidth of the SAW resonator 300 may be reduced, and thus the thickness of the insulating layer 360 is preferably such that the bandwidth of the SAW resonator 300 is not affected.
[0088] On the other hand, the insulating layer 360 formed between the IDT electrode 350 and the piezoelectric substrate 310 may be formed as follows: Figure 6 The insulating layer 360 can be formed only directly below the seed layer 320 , and the insulating layer 360 under the adjacent IDT electrodes 350 can be separated from each other by removing the insulating layer 360 between the adjacent IDT electrodes.
[0089] In addition, the IDT electrode 350 may also be formed as Figure 5 The dual structure of the lower main electrode layer 231 and the upper main electrode layer 232 is shown in FIG.
[0090] Figure 7 FIG. 1 is a diagram of a SAW resonator with an improved electrode structure according to yet another embodiment of the present invention. It can be understood that, as before, the SAW resonator has the same structure as the electrode structure of the SAW resonator. Figure 2a and Figure 5 Constituent elements with similar reference numerals in the described embodiments are corresponding constituent elements, and detailed descriptions thereof will be omitted.
[0091] Reference Figure 7 At least one of the IDT electrodes 450 of the SAW resonator 400 having an improved electrode structure according to still another embodiment of the present invention may be a contact electrode having a wiring layer 480 formed on an upper portion.
[0092] The IDT electrode 450 may further include an ohmic contact layer 470 formed on the main electrode layer 430 . The ohmic contact layer 470 may prevent oxidation of the main electrode layer 430 and reduce contact loss with the wiring layer 480 formed on the IDT electrode 450 .
[0093] Specifically, the ohmic contact layer 470 may include a substance having a low diffusion coefficient or a low ionization tendency, such as titanium, silver, gold, and platinum, and in some embodiments, the ohmic contact layer 470 may include the same substance as the seed layer 420 and the lower wiring layer 481. Preferably, the ohmic contact layer 470 may include titanium, which is relatively inexpensive and has a sufficient tunneling effect.
[0094] When the main electrode layer 430 including aluminum or the like is exposed to the uppermost portion of the IDT electrode 450, the main electrode layer 430 naturally generates oxide (e.g., aluminum oxide (Al2O3)), which, when combined with the wiring layer 480, forms a capacitive contact rather than an ohmic contact, thereby increasing contact loss and reducing performance.
[0095] Therefore, the SAW resonator 400 according to the present embodiment forms the ohmic contact layer 470 at the uppermost end of the IDT electrode 450, thereby reducing the contact loss with the wiring layer 480. In other words, the ohmic contact layer 470 is generated by, for example, the same titanium as the lower wiring layer 481, and the titanium oxide in the ohmic contact layer 470 formed by natural oxidation of titanium minimizes the contact resistance when combined with the lower wiring layer 481 containing titanium to prevent performance degradation due to contact loss. This is because oxygen diffuses from the titanium oxide of the ohmic contact layer 470 to the lower wiring layer 481, thereby minimizing the contact resistance.
[0096] Figure 8 and Fig. 9 It is used to explain the Figure 7 FIG. 4 is a diagram of the effect of the SAW resonator 400 of the embodiment.
[0097] Reference Figure 8 ,like Figure 7 As shown in the embodiment of Figure 8 The results of forming ohmic contact and capacitive contact are shown separately.
[0098] Reference Fig. 9 , shows a graph comparing the passband attenuation when the bonding metal layer 370 is formed (green graph) and when the bonding metal layer is not formed (cyan graph). It can be confirmed that when the bonding metal layer 370 is formed, the loss is reduced by about 0.2 to 0.4 dB compared to the case where the bonding metal layer 370 is not formed.
[0099] Fig.10 FIG. 1 is a sequence diagram for explaining a method for manufacturing a SAW resonator having an improved electrode structure according to an embodiment of the present invention.
[0100] Reference Fig.10 According to an embodiment of the present invention, a method for manufacturing a SAW resonator with an improved electrode structure may include the following steps: preparing a piezoelectric substrate S110; performing surface treatment on the surface of the substrate by ion implantation or plasma S120; forming an IDT electrode film including a seed layer and a main electrode layer S130; and forming an IDT electrode by etching the IDT electrode film S140.
[0101] Figures 11 to 16 FIG. 1 is a diagram for explaining an intermediate step of a method for manufacturing a SAW resonator having an improved electrode structure according to an embodiment of the present invention.
[0102] Reference Fig.11 , a piezoelectric substrate 110 in which a support substrate 111, an energy confinement layer 112, and a piezoelectric layer 113 are sequentially stacked is provided (S110). The piezoelectric substrate 110 may be formed by bonding two or more wafers including at least a portion of the support substrate 111, the energy confinement layer 112, and the piezoelectric layer 113, for example, but the present invention is not limited thereto.
[0103] Reference Fig.12 , a step S120 of performing a surface treatment P on the surface of the piezoelectric layer 113 by ion implantation or plasma is performed.
[0104] In order to perform plasma surface treatment of the piezoelectric layer 113, plasma can be generated using at least any one of, for example, argon (Ar), oxygen (O2), nitrogen (N2), ammonia (NH3), neon (Ne) and xenon (Xe). Preferably, a gas such as argon (Ar) can be used that is in an ionized gas state without using a solvent and that can control the depth of the amorphous layer on the surface of the piezoelectric layer 113 generated by the surface treatment so that it does not become too large.
[0105] On the other hand, the surface treatment of the piezoelectric layer 113 may be performed by implanting hydrogen or helium ions into the piezoelectric layer 113 to form an amorphous layer on the surface.
[0106] In some embodiments, before performing the surface treatment P step, a process of removing surface contaminants of the piezoelectric layer 113 by wet cleaning or the like may be performed.
[0107] Reference Fig.13 , performing a step of forming a seed layer 121 on the piezoelectric layer 113. The seed layer 121 may include, for example, titanium, magnesium, zinc, cadmium, scandium, and ruthenium generated by RF sputtering. In some embodiments of the present invention, the seed layer 121 may be formed to be less than 10 nm.
[0108] Reference Fig.14 , a step of forming an IDT electrode film 151 by stacking a main electrode layer 131 on the seed layer 121 is performed. The base metal layer 131 can be formed by RF sputtering at least any one of materials such as copper, silver, gold, platinum and tungsten, and the main electrode layer 141 can be formed by RF sputtering a material having a lower density than the metal material constituting the base metal layer 131 such as aluminum.
[0109] In some embodiments of the present invention, Fig.15 As shown in FIG. 1 , the main electrode layer can also be divided into a lower main electrode layer 131 and an upper main electrode layer 141. In other words, Figure 5 As in the SAW resonator 200 in the illustrated embodiment, a structure in which a lower main electrode layer 231 and an upper main electrode layer 232 are stacked is formed on the seed layer 220. At this time, the lower main electrode layer 131 can be formed by RF sputtering at least any one of materials such as copper, silver, gold, platinum and tungsten, and the upper main electrode layer 141 can be formed by RF sputtering a material having a lower density than a metal material constituting the lower main electrode layer 131 such as aluminum.
[0110] Reference Fig.16 , performing a step of forming a resist pattern 152 on the main electrode layer 141. Forming the resist pattern 152 may include, for example, forming a photoresist on the main electrode layer 141, and patterning the photoresist formed by exposure and development to selectively expose a portion of the surface of the main electrode layer 141.
[0111] Next, refer to Figure 2a, performing a step of forming an IDT electrode 150 by etching the IDT electrode film 151. Forming the IDT electrode 150 may include etching the IDT electrode film 151 by using the resist pattern 152 as an etching mask. Since the seed layer 121, the base metal layer 131, and the main electrode layer 141 constituting the IDT electrode film 151 are respectively composed of different materials, their etching processes are also performed differently. For example, if the seed layer 121 is titanium, Cl2 and CCl4 can be used for the etching process. If the base metal layer 131 is tungsten, NF3, SF6, CF4, and Cl2 can be used for the etching process. If the main electrode layer 141 is aluminum, Cl2 and BCl2 gases can be used for the etching process.
[0112] In some embodiments of the present invention, Figure 5 As shown, when the insulating layer 260 is interposed under the IDT electrode 250 , in order to expose the surface of the piezoelectric layer 213 , a process of etching the insulating layer 260 using a fluorine-based gas may be added.
[0113] Fig.17 FIG. 1 is a sequence diagram for explaining a method for manufacturing a SAW resonator having an improved electrode structure according to another embodiment of the present invention. Fig.17 Corresponds to Figure 6 A method for manufacturing the SAW resonator 30 is shown in the embodiment.
[0114] Reference Fig.17 According to another embodiment of the present invention, a method for manufacturing a SAW resonator includes the following steps: preparing a supporting substrate on which an energy confinement layer and a piezoelectric layer are stacked in sequence S210; performing surface treatment on the surface of the piezoelectric layer by ion implantation or plasma S220; forming an IDT electrode film including a seed layer and a main electrode layer S230; forming an ohmic contact layer on the IDT electrode film S240; and etching the ohmic contact layer and the IDT electrode film to form an IDT electrode formed on the upper part of the bonding metal layer S250. Figure 8 The difference from the manufacturing method described above is that after an ohmic contact layer is additionally formed on the IDT electrode film, the bonding metal layer and the IDT electrode film are etched to form the IDT electrode formed on the bonding metal layer.
[0115] Fig.18 and Fig.19 FIG. 1 is a diagram for explaining an intermediate step of a method for manufacturing a SAW resonator having an improved electrode structure according to another embodiment of the present invention. In the previously described embodiment, since the processes up to the formation of the IDT electrode film 151 are the same, the description thereof is omitted.
[0116] Reference Fig.18, an ohmic contact layer 471 is formed on the IDT electrode film 451 S240. The ohmic contact layer 471 may include titanium formed by sputtering, for example, the same as the lower wiring layer 481. If the lower wiring layer 481 is formed of titanium, the lower wiring layer 381 may be composed of titanium oxide by natural oxidation.
[0117] Reference Fig.19 and Figure 7 , a step of forming a resist pattern 452 on the ohmic contact layer 471 and etching the ohmic contact layer 471 and the IDT electrode film 451 by using the resist pattern 452 as an etching mask may be performed.
[0118] Although the embodiments of the present invention are described above with reference to the accompanying drawings, it is understood that a person having general knowledge in the technical field to which the present invention belongs can implement the present invention in other specific forms without changing the technical ideas or essential features of the present invention. Therefore, it should be understood that the embodiments described above are exemplary in all aspects and are not restrictive.
Claims
1. A SAW resonator having an electrode structure with improved performance, characterized in that: include: Piezoelectric substrate; as well as A plurality of IDT electrodes are formed on the piezoelectric substrate. The multiple IDT electrodes include: A seed layer laminated on the surface of the piezoelectric body; as well as a main electrode layer formed on the seed layer, An amorphous layer is formed on the upper surface of the piezoelectric layer.
2. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: At least one of the plurality of IDT electrodes is a contact electrode, The contact electrode further includes an ohmic contact layer formed on the main electrode layer.
3. The SAW resonator with an electrode structure having improved performance according to claim 2, characterized in that: Also includes: a wiring layer formed on the ohmic contact layer and joined to the contact electrode, and including a lower wiring layer, The ohmic contact layer and the lower wiring layer form an ohmic contact.
4. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: The ohmic contact layer includes titanium, titanium nitride (TiN), titanium oxide (TiOx), and titanium-tungsten (TiW).
5. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: The main electrode layer includes a lower main electrode layer and an upper main electrode layer which are sequentially stacked.
6. The SAW resonator with an electrode structure having improved performance according to claim 5, characterized in that: The lower main electrode layer includes a metal having a higher density than that of the upper main electrode layer.
7. The SAW resonator with an electrode structure having improved performance according to claim 6, characterized in that: The lower main electrode layer includes at least one of tungsten (W) or copper (Cu), The upper main electrode layer includes aluminum (Al).
8. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: The piezoelectric substrate includes: A supporting substrate; an energy confinement layer formed on a supporting substrate; and a piezoelectric layer formed on the energy confinement layer, The energy limiting layers include: A low speed layer and / or a high speed layer.
9. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: The seed layer includes at least any one of titanium, titanium nitride (TiN), titanium oxide (TiOx), titanium-tungsten (TiW), and chromium (Cr).
10. The SAW resonator with an electrode structure having improved performance according to claim 1, characterized in that: An insulating layer is further included between the plurality of IDT electrodes and the amorphous layer.
11. A method for manufacturing a SAW resonator having an electrode structure with improved performance, characterized in that: The steps include: preparing a piezoelectric substrate; The surface of the piezoelectric substrate is subjected to surface treatment by ion implantation or plasma to form an amorphous layer; forming a seed layer on the amorphous layer; forming a main electrode layer on the seed layer; as well as The seed layer and the main electrode layer are etched to form a plurality of IDT electrodes.
12. The method for manufacturing a SAW resonator having an electrode structure with improved performance according to claim 11, characterized in that: The method further includes forming an ohmic contact layer on the main electrode layer before forming a plurality of IDT electrodes.
13. The method for manufacturing a SAW resonator having an electrode structure with improved performance according to claim 12, characterized in that: After the step of forming a plurality of IDT electrodes, the method further includes forming a wiring layer on the ohmic contact layer so as to be connected to a contact electrode of one of the plurality of IDT electrodes. The ohmic contact layer and the wiring layer form an ohmic contact.
14. The method for manufacturing a SAW resonator having an electrode structure with improved performance according to claim 11, characterized in that: The method further includes forming an insulating layer between the seed layer and the amorphous layer before forming the plurality of IDT electrodes.
15. The method for manufacturing a SAW resonator having an electrode structure with improved performance according to claim 11, characterized in that: The step of forming the main electrode layer includes the step of sequentially stacking a lower main electrode layer and an upper main electrode layer, The lower main electrode layer includes a material having a higher density than the upper main electrode layer.
16. The SAW resonator with an electrode structure having improved performance according to claim 15, characterized in that: The lower main electrode layer includes at least one of tungsten (W) or copper (Cu), The upper main electrode layer includes aluminum (Al).
17. The method for manufacturing a SAW resonator having an electrode structure with improved performance according to claim 12, characterized in that: The bonding metal layer includes titanium, titanium nitride (TiN), titanium oxide (TiOx), and titanium-tungsten (TiW).