Silver-based metal powder and method for producing silver-based metal powder
By controlling the content of impurity elements and using atomization methods to produce silver-based metal powders, the problem of unstable sintering of silver-based metal powders at low temperatures and high dew point atmospheres is solved, and stable sintering and calcination are achieved, which is suitable for powder metallurgy and conductive slurries. Material.
Patent Information
- Application Number
- CN202280092075.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-10-01
AI Technical Summary
Silver-based metal powder cannot be sintered stably in an atmosphere with low temperature and high dew point, and the size and strength of the sintered body are prone to deviations.
By controlling the total content of impurity elements below 500ppm, ensuring that the standard free energy of formation of the oxide in the temperature range below 600°C is below silicon dioxide, and the mixing enthalpy with silver is below aluminum, the atomization method is used to manufacture the silver system Metal powder reduces the oxidation of impurity elements and improves sintering stability.
Stable sintering and calcination of silver-based metal powder is achieved in a low-temperature, high-dew-point atmosphere, reducing the size and strength deviation of the sintered body, and is suitable for powder metallurgy and conductive slurry materials.
Smart Images

Figure BDA0004999083370000071 
Figure BDA0004999083370000081 
Figure BDA0004999083370000091
Abstract
Description
Technical Field
[0001] The present invention relates to a silver-based metal powder. Specifically, the silver-based metal powder can be stably sintered and calcined even in a low-temperature or high-dew-point atmosphere, and has little variation in strength and size of the sintered body, so it can be suitably used as a raw material powder for powder metallurgy or a raw material powder for a conductive paste material. Background Art
[0002] Silver exhibits excellent electrical conductivity, thermal conductivity, oxidation resistance, and corrosion resistance, and is also very popular as a precious metal for use in clothing items. Therefore, silver-based metal powders consisting of silver and silver alloys have been used as raw material powders for metal powder injection molding or silver clay.
[0003] In recent years, the use of silver-based metal powders as raw material powders of calcined or thermosetting conductive pastes has also been expanding in the field of electronic materials.
[0004] Silver is a precious metal that is difficult to oxidize. In addition, since silver oxide is easily decomposed, it has the excellent property that it does not require a reducing atmosphere as long as the temperature is raised to a sufficient level, and can be sintered even in an atmosphere with a high oxygen partial pressure such as the air atmosphere.
[0005] However, from the perspective of manufacturing cost, a silver-based metal powder is desired that has a sintering temperature as low as possible and can be sintered even in an atmosphere with harsh conditions such as a high dew point. However, there is the following problem: even silver-based metal powder cannot be stably sintered in an atmosphere with a low temperature and a high dew point, and problems such as deviations in the size and strength of the sintered body are likely to occur.
[0006] Therefore, it is desired to develop a silver-based metal powder that can be stably sintered even in a low-temperature, high-dew-point atmosphere and that does not easily cause variations in the size and strength of the sintered body.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent document 1: Japanese Patent Application Laid-Open No. 2001-3101. Summary of the invention
[0010] Problems to be solved by the invention
[0011] Patent Document 1 discloses a silver powder for silver clay, which contains 20 ppm to 900 ppm in total of one or more of tin, lead, copper, bismuth, and iron, and improves sinterability by intentionally adding these elements.
[0012] However, since the sintering temperature of the silver powder in Patent Document 1 is 900° C., there is no description on the stability during sintering in a low-temperature, high-dew-point atmosphere.
[0013] The inventors have made solving the above-mentioned various problems a technical issue, and have repeatedly conducted intensive experiments focusing on impurity elements in silver and silver alloys. As a result, they surprisingly found that if the following silver-based metal powder is used, it can be stably sintered and calcined even in a low-temperature, high-dew-point atmosphere, and the strength and dimensional deviations of the sintered body can be suppressed, thereby solving the above-mentioned technical problems: the total content of impurity elements contained in the silver-based metal powder is less than 500 ppm, and with respect to the impurity elements, the standard formation free energy of the oxide in the temperature range below 600°C is less than the standard formation free energy of silicon dioxide in the said temperature range, and the mixing enthalpy with silver is less than that of aluminum.
[0014] Technical solutions to problems
[0015] The above technical problems can be solved by the following present invention.
[0016] The present invention provides a silver-based metal powder, wherein the total content of impurity elements contained in the silver-based metal powder is less than 500 ppm, and with respect to the impurity elements, the standard formation free energy of the oxide in a temperature range below 600°C is less than the standard formation free energy of silicon dioxide in the temperature range, and the mixing enthalpy with silver is less than that of aluminum.
[0017] Furthermore, the present invention provides the silver-based metal powder in which the total content of the rare earth elements as the impurity elements is 100 ppm or less.
[0018] Furthermore, the present invention provides the silver-based metal powder, wherein the content of lithium as the impurity element is 100 ppm or less.
[0019] Furthermore, the present invention provides the silver-based metal powder, wherein the total content of calcium and / or magnesium as the impurity elements is 300 ppm or less.
[0020] Furthermore, the present invention provides the silver-based metal powder, wherein the content of zirconium as the impurity element is 300 ppm or less.
[0021] Furthermore, the present invention provides the silver-based metal powder, wherein the content of silicon as the impurity element is 300 ppm or less.
[0022] Furthermore, the present invention provides the silver-based metal powder, wherein the content of aluminum as the impurity element is 300 ppm or less.
[0023] Furthermore, the present invention is a method for producing the silver-based metal powder by an atomization method.
[0024] Effects of the Invention
[0025] In the silver-based metal powder of the present invention, the standard formation free energy of the oxide in the temperature range below 600°C is lower than the standard formation free energy of silicon dioxide in the said temperature range, and the total content of impurity elements whose mixing enthalpy with silver is lower than that of aluminum is lower than 500 ppm. Therefore, even in a low-temperature, high-dew-point atmosphere, stable sintering and calcination can be performed, and the deviation in the size and strength of the sintered body is small. Therefore, it can be appropriately used as a raw powder for powder metallurgy purposes or a raw powder for conductive paste materials. DETAILED DESCRIPTION
[0026] The present invention relates to silver-based metal powder composed of silver and / or silver alloy.
[0027] In the silver-based metal powder of the present invention, the total content of the following impurity elements (hereinafter sometimes referred to as "specific impurity elements") is less than 500 ppm: the standard free energy of formation of the oxide in the temperature range below 600°C is less than the standard free energy of formation of silicon dioxide in the said temperature range, and the mixing enthalpy with silver is less than that of aluminum.
[0028] It is believed that the standard formation free energy of oxides in the temperature range below 600°C is the standard formation free energy of silicon dioxide in the said temperature range. Impurity elements below this temperature tend to be easily oxidized in the temperature range below 600°C. When these elements exist in trace amounts on the surface of powder particles or in powder particles, they will preferentially react with oxygen in the atmosphere to form oxides.
[0029] It is also believed that the mixing enthalpy is a thermodynamic value that indicates the magnitude of the interaction between elements, and there is a tendency that the smaller the value, the easier it is for the elements to bond with each other. However, since the impurity elements whose mixing enthalpy with silver is lower than that of aluminum have a high affinity for silver, they do not separate from silver and locally form oxides, but instead form oxides in a state of uniformly coating the surface of the powder particles of the silver-based metal or uniformly dispersed in the particles.
[0030] The oxide of the specific impurity element has little influence on sintering when the sintering temperature is sufficiently high or in a favorable atmosphere such as a reducing atmosphere or an inert atmosphere with a low dew point.
[0031] However, it is speculated that in harsh atmospheres such as low temperature or high dew point atmospheres, the solid phase diffusion of silver, the main component, on the particle surface or in the particles is hindered, so the sintering progress is delayed or uneven, resulting in poor sintering and deviations in the size or strength of the sintered body.
[0032] The total content of the specific impurity elements in the present invention is 500 ppm or less.
[0033] This is because when the total content of the specific impurity elements exceeds 500 ppm, sintering and calcination become unstable, so that the size and strength of the sintered body may vary.
[0034] In addition, the "total content" in the present invention refers to the content of all specific impurity elements contained in the silver-based metal powder in total.
[0035] Examples of specific impurity elements include rare earth elements represented by yttrium (Y) and neodymium (Nd), lithium (Li), calcium (Ca), magnesium (Mg), zirconium (Zr), silicon (Si), and aluminum (Al).
[0036] The standard free energy of formation of the oxide in a temperature range of 600° C. or less and the mixing enthalpy with silver may be determined by using the values described in the literature.
[0037] The literature value of the standard free energy of formation of silicon dioxide at 600°C is -750 (kJ / mol-O2), and the literature value of the mixing enthalpy of aluminum and silver is -4 (kJ / mol).
[0038] In the present invention, the total content of rare earth elements as specific impurity elements is preferably 100 ppm or less.
[0039] This is because rare earth elements are elements that have a large influence on inhibiting stable sintering.
[0040] The content of lithium as a specific impurity element is preferably 100 ppm or less.
[0041] This is because lithium is an element that has a significant influence on inhibiting stable sintering.
[0042] The total content of calcium and / or magnesium as specific impurity elements is preferably 300 ppm or less.
[0043] The content of zirconium as a specific impurity element is preferably 300 ppm or less.
[0044] The content of silicon as a specific impurity element is preferably 300 ppm or less.
[0045] The content of aluminum as a specific impurity element is preferably 300 ppm or less.
[0046] This is because calcium, magnesium, zirconium, silicon, and aluminum have less influence than rare earth elements or lithium, but they hinder stable sintering.
[0047] The specific impurity elements can be analyzed and quantified by ICP emission spectrometry on a solution obtained by dissolving silver-based metal powder in an acid.
[0048] In the present invention, an element whose standard free energy of formation of oxide in a temperature range of 600° C. or less is higher than that of silicon dioxide in the above temperature range, or an impurity element whose mixing enthalpy with silver is higher than that of aluminum may be contained.
[0049] As an element whose standard free energy of formation of an oxide in a temperature range below 600°C is higher than the standard free energy of formation of silicon dioxide in the said temperature range, palladium (Pd) is exemplified; as an element whose mixing enthalpy with silver is greater than that of aluminum, titanium (Ti) is exemplified; as an element whose standard free energy of formation of an oxide in a temperature range below 600°C is higher than the standard free energy of formation of silicon dioxide in the said temperature range and whose mixing enthalpy with silver is greater than that of aluminum, nickel (Ni), copper (Cu) and iron (Fe) are exemplified.
[0050] The silver-based metal powder of the present invention may contain a silver-copper alloy or a silver-palladium alloy used as a brazing filler metal.
[0051] The method for producing the silver-based metal powder of the present invention is not particularly limited, but it is preferably produced by an atomization method.
[0052] This is because the atomization method is relatively cheap and efficient, and can produce silver-based metal powder in large quantities.
[0053] The atomization method is not limited, and may be a known method such as water atomization, gas atomization, centrifugal atomization, etc.
[0054] Furthermore, in the present invention, the total content of specific impurity elements needs to be controlled below 500 ppm, and therefore attention needs to be paid to the silver ingot used as the raw material. However, since the specific impurity elements in the present invention are basically easily oxidized, when melted in an atmosphere with a certain degree of oxygen, oxides are formed, which can be separated from the solution of silver and silver alloy and removed.
[0055] Therefore, the total content of specific impurity elements in the ingot state before melting does not need to be 500 ppm or less.
[0056] The average particle size of the silver-based metal powder of the present invention is not limited and may be appropriately determined as needed.
[0057] Generally, the average particle size of silver-based metal powders used in the field of electronic materials is 50 μm or less. From the viewpoint of forming a fine circuit pattern, the average particle size is preferably 10 μm or less.
[0058] When producing fine powders having an average particle size of 10 μm or less, the fine powders can be produced by a water atomization method which is easy to finely pulverize from the viewpoint of yield.
[0059] The average particle size of the silver-based metal powder can be measured using a laser diffraction particle size distribution analyzer.
[0060] [Example]
[0061] Although the examples and comparative examples of the present invention are shown, the present invention is not limited thereto.
[0062] (Powder production)
[0063] After a raw material high-purity silver ingot (99.99% or more) is heated and melted, each impurity element listed in Tables 1 to 3 is appropriately added to adjust the composition.
[0064] Each silver-based metal powder was obtained by a water atomization method in which high-pressure water was sprayed onto the molten solution while the solution was freely dropped to disperse the solution and then rapidly condensed and solidified.
[0065] Coarse particles were removed from each of the obtained silver-based metal powders using a 100-mesh sieve.
[0066] (Measurement of average particle size)
[0067] The average particle size of each silver-based metal powder was measured using a laser diffraction particle size distribution analyzer MT3000II (manufactured by MicrotracBEL Co., Ltd.).
[0068] The "average particle size" in the present invention refers to the cumulative 50% particle size (D 50 path).
[0069] (Quantification of impurity elements in silver-based metal powder)
[0070] After each of the obtained silver-based metal powders was dissolved in acid to form a solution, the content of each impurity element was measured using an ICP emission spectrometer iCAP7600 (manufactured by Thermo Fisher Scientific).
[0071] The blank columns in Tables 1 to 3 indicate that the concentration is less than the detection limit of 10 ppm.
[0072] Qualitative analysis based on fluorescent X-rays was performed on each of the obtained silver-based metal powders using ZSX Primus IV (manufactured by Rigaku Corporation), and it was confirmed that no peaks of elements other than the elements listed in Tables 1 to 3 were detected.
[0073] (Evaluation of Sinterability)
[0074] In each silver-based metal powder of the embodiment and the comparative example, zinc stearate was used as a lubricant for die lubrication, and the powder compaction density was 7.7 g / cm 3The resultant was molded into a Φ14-7×5 mm cylindrical shape and maintained at 400°C for 15 minutes in a pure nitrogen atmosphere with a dew point of 0°C to obtain a sintered body.
[0075] The radial crushing strength of each of the obtained sintered bodies was measured in accordance with JIS Z 2507 using AUTOGRAPH AG-IS 50 kN (manufactured by Shimadzu Corporation).
[0076] The sinterability of each powder was evaluated with n number: 5. If all the measured radial crushing strengths were 120 MPa or more, the sinterability was evaluated as ◎, if they were 100 MPa or more, the sinterability was evaluated as 0, and if none was less than 100 MPa, the sinterability was evaluated as ×.
[0077] [Table 1]
[0078]
[0079] [Table 2]
[0080]
[0081] [Table 3]
[0082]
[0083] By comparing Examples 1 to 9 and Comparative Examples 1 to 3 shown in Table 1, it was confirmed that the sinterability was stable when the total content of yttrium (Y) and neodymium (Nd) classified as rare earth elements was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. In addition, it was confirmed that the sinterability was particularly stable when it was 100 ppm or less.
[0084] In addition, by comparing Examples 10 to 12 and Comparative Example 4 shown in Table 1, it was confirmed that the sinterability was stable when the lithium (Li) content was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. Furthermore, it was confirmed that the sinterability was particularly stable when it was 100 ppm or less.
[0085] In addition, by comparing Examples 13 to 21 and Comparative Examples 5 to 7 shown in Table 2, it was confirmed that the sinterability was stable when the total content of calcium (Ca) and magnesium (Mg) was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. Furthermore, it was confirmed that the sinterability was particularly stable when it was 300 ppm or less.
[0086] In addition, by comparing Examples 22 to 24 and Comparative Example 8 shown in Table 2, it was confirmed that the sinterability was stable when the zirconium (Zr) content was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. Furthermore, it was confirmed that the sinterability was particularly stable when it was 300 ppm or less.
[0087] In addition, by comparing Examples 25 to 27 and Comparative Example 9 shown in Table 3, it was confirmed that the sinterability was stable when the silicon (Si) content was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. Furthermore, it was confirmed that the sinterability was particularly stable when it was 300 ppm or less.
[0088] In addition, by comparing Examples 28 to 30 and Comparative Example 10 shown in Table 3, it was confirmed that the sinterability was stable when the aluminum (Al) content was 500 ppm or less, and the stability decreased when it exceeded 500 ppm. Furthermore, it was confirmed that the sinterability was particularly stable when it was 300 ppm or less.
[0089] In addition, by comparing Examples 31 to 34 and Comparative Examples 11 to 14 shown in Table 3, it was confirmed that when the standard free energy of formation of the oxide in a temperature range below 600°C is lower than the standard free energy of formation of silicon dioxide in the same temperature range as the temperature range and the total content of impurity elements whose mixing enthalpy with silver is lower than that of aluminum is lower than 500 ppm, the sintering property is stable, and when it exceeds 500 ppm, the stability is reduced.
[0090] Industrial Applicability
[0091] In the silver-based metal powder of the present invention, the standard formation free energy of the oxide in the temperature range below 600°C is lower than the standard formation free energy of silicon dioxide in the said temperature range, and the total content of impurity elements whose mixing enthalpy with silver is lower than that of aluminum is lower than 500 ppm. Therefore, even in a low-temperature, high-dew-point atmosphere, stable sintering and calcination can be performed, and the strength and dimensional deviations of the sintered body are small. Therefore, it can be appropriately used as a raw material powder for powder metallurgy purposes or a raw material powder for conductive paste materials.
[0092] Therefore, the present invention has high industrial applicability.
Claims
1. A silver-based metal powder, in, The total content of impurity elements contained in the silver-based metal powder is less than 500 ppm. As for the impurity elements, the standard formation free energy of the oxide in the temperature range below 600°C is lower than the standard formation free energy of silicon dioxide in the temperature range, and the mixing enthalpy with silver is lower than that of aluminum.
2. The silver-based metal powder according to claim 1, in, The total content of the rare earth elements as the impurity elements is 100 ppm or less.
3. The silver-based metal powder according to claim 1, in, The content of lithium as the impurity element is 100 ppm or less.
4. The silver-based metal powder according to claim 1, in, The total content of calcium and / or magnesium as the impurity elements is 300 ppm or less.
5. The silver-based metal powder according to claim 1, in, The content of zirconium as the impurity element is 300 ppm or less.
6. The silver-based metal powder according to claim 1, in, The content of silicon as the impurity element is 300 ppm or less.
7. The silver-based metal powder according to claim 1, in, The content of aluminum as the impurity element is 300 ppm or less.
8. The method for producing a silver-based metal powder according to claims 1 to 7, in, Produced by atomization.
Citation Information
Patent Citations
Covering-type copper-nickel-silver composite powder and preparation method thereof
CN102873324A
Spherical silver powder and method for producing same
CN104136151A
Low-temperature dispersion-based syntheses of silver and silver products produced thereby
CN104685076A
Solvent-free syntheses of silver and silver products produced thereby
CN104884193A
Silver powder and production method thereof
CN111132777A