Method for producing electrode for electrochemical cell, composite electrode and electrochemical cell

By combining self-supporting electrode films or dry electrode mixtures with porous collector foils and pressing them to form composite electrodes, the problems of high cost and consumption in the manufacturing of existing electrodes for electrochemical monomers are solved, and the energy density and mechanical stability are improved. Simplified manufacturing process.

CN118743041APending Publication Date: 2024-10-01BAYERISCHE MOTOREN WERKE AG
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380023295.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-14
Filing Date
2023-02-22
Publication Date
2024-10-01

Smart Images

  • Figure CN118743041A_ABST
    Figure CN118743041A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing an electrode for an electrochemical cell, comprising the following steps: first, providing a self-supporting electrode film (30) and / or a dry electrode mixture comprising a plurality of dry-treated particles, the plurality of dry treated particles include a binder, a conductive additive, and an active material. Furthermore, a porous current collector foil (22) is provided, the porous current collector foil (22) having openings (24) extending through the porous current collector foil (22). A self-supporting electrode film (30) and / or a dry electrode mixture is applied and pressed onto a porous current collector foil (22) to form the composite electrode (20), the electrode film (30) and / or the dry electrode mixture being pressed at least partially into openings (24) of the porous current collector foil (22), and the composite electrode (30) being free of an adhesion promoter. The invention further relates to a composite electrode (20) obtained in this way and to an electrochemical cell having such a composite electrode (20).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing an electrode for an electrochemical cell, a composite electrode obtainable according to the method and an electrochemical cell having such a composite electrode. Background Art

[0002] Methods are known for producing electrodes for electrochemical cells, in which a solvent-based coating composition (so-called "slurry"), which contains an electrochemically active material, a binder and additives such as conductive additives, as well as a carrier solvent, is applied to a collector foil. A subsequent drying step is required, since the slurry usually additionally contains a solvent such as N-methyl-2-pyrrolidone (NMP), which must be removed to prevent it from remaining in the electrode or in an electrochemical cell having such an electrode. Therefore, these solvents must be removed after the coating process is completed before the electrode can be installed in the electrochemical cell. Therefore, wet chemical electrode production methods are associated with additional costs and considerable expenditure. Therefore, for example, the carrier solvent must be distilled, condensed and cleaned. This requires a large amount of logistics and energy expenditure.

[0003] US2013 / 0157141A1 discloses a method for producing a self-supporting electrode, which forgoes the use of a carrier solvent. To this end, dry and free-flowing particles containing active materials, binders and additives (e.g. conductive carbon black, also referred to as "carbon black" in industrial terms) are mixed with each other and processed into a self-supporting, i.e. self-stable electrode film. As a binder, in particular "fibrillable" polymers such as polytetrafluoroethylene (PFTE) are used. The self-supporting electrode is then applied to a metal collector foil, such as a rolled aluminum foil, which has been etched in advance and provided with an adhesion promoter layer (also referred to as "primer coating").

[0004] The disadvantage of this method is that an adhesion promoter must be used between the self-supporting electrode film and the collector foil in order to produce a sufficiently stable connection or adhesion between the electrode film and the collector foil. The resulting additional coating acts as dead material in the electrochemical cell using such an electrode and thus reduces the volumetric energy density and gravimetric energy density of the electrochemical cell.

[0005] Furthermore, the application of the adhesion promoter is usually carried out wet-chemically and / or requires wet-chemical etching or other pretreatment of the collector foil. In addition, the self-supporting electrode film must be hot-laminated onto the collector foil in order to achieve adequate adhesion. Therefore, a number of cost-intensive and time-consuming steps are also required, which must in part be carried out wet-chemically. Summary of the invention

[0006] The object of the present invention is to provide a possibility for further reducing the production effort and costs of electrodes for electrochemical cells. In particular, it should be possible to dispense with wet chemical processes or at least reduce their number. Preferably, wet painting and / or hot lamination for applying a primer coating should be omitted.

[0007] This object is achieved by a method for producing an electrode for an electrochemical cell, the method comprising the following steps: first, a self-supporting electrode film and / or a dry electrode mixture is provided, the self-supporting electrode film and / or the dry electrode mixture comprising a plurality of dry-processed particles, the plurality of dry-processed particles comprising at least one binder, a conductive additive and an active material. In addition, a porous collector foil is provided, the porous collector foil having an opening extending through the porous collector foil. The self-supporting electrode film and / or the dry electrode mixture is applied and pressed onto the porous collector foil to form a composite electrode, wherein the electrode film and / or the dry electrode mixture is at least partially pressed into the opening of the porous collector foil, and the composite electrode does not contain an adhesion promoter.

[0008] A “self-supporting electrode film” is to be understood here and hereinafter as a dimensionally stable, in particular self-stable, electrode film which can be handled on its own, ie does not have to be applied to an additional carrier material, in particular does not have to have been applied to a collector foil.

[0009] A "dry electrode mixture" refers here and hereinafter to a mixture comprising a plurality of dry-processed particles, which does not have a self-stable form per se but is directly pressed (eg rolled or calendered) into a porous current collector foil to obtain a composite electrode.

[0010] This enables the dry electrode mix to be rolled or calendared directly into a porous current collector, with the porous current collector in the resulting composite electrode being either centrally or asymmetrically oriented in the composite electrode.

[0011] For a particularly simple design of the method, in particular either a self-supporting electrode membrane or a dry electrode mixture is used.

[0012] The self-supporting electrode membrane is produced in particular according to the method for producing a self-supporting electrode membrane as described in US 2013 / 0157141 A1.

[0013] The components used in the dry electrode mixture may be the same as those used for preparing the self-supporting electrode membrane according to US 2013 / 0157141 A1.

[0014] The types of (electrode) binders, conductive additives and active materials in the electrode film are not further restricted as long as a self-supporting electrode film or a dry electrode mixture can be produced from these materials.

[0015] In one embodiment, the electrode film has a thickness of 0.5 g / cm 3 or higher density.

[0016] If the composite electrode is an anode, the electrode film in one embodiment contains 30 to 98 wt % of graphite, 70 wt % or less of silicon, 9 wt % or less of carbon black and 0.5 to 10 wt % of a binder (respectively relative to the total weight of the electrode film).

[0017] A collector foil is a metallic, metal-containing or at least electrically conductive carrier foil which can serve as a current collector in a composite electrode.

[0018] If the electrode obtained in the production method according to the invention is a cathode, aluminum expanded metal (produced, for example, by Bender GmbH, Germany) is particularly suitable.

[0019] The term “composite electrode” refers to an electrode produced by means of the method according to the invention and a composite consisting of a collector foil and an electrode film applied to the collector foil or pressed together with the collector foil, which thus serves as an electrode coating for the collector foil.

[0020] According to the invention, the composite electrode and in particular the porous collector foil do not contain an adhesion promoter. This means that the composite electrode does not have a primer coating as known in the prior art. In this way, no additional method steps are required to apply such a primer coating containing an adhesion promoter. As a result, in particular the known wet chemical processes for applying the primer coating and the process costs are avoided.

[0021] It has been found that by using a porous collector foil, it is possible to dispense with an additional adhesion promoter and nevertheless achieve a sufficiently stable and reliable connection between the electrode film formed from the dry-processed particles and the collector foil. Thus, any pretreatment steps that would have to be carried out in order to be able to apply an adhesion promoter to the collector foil are also dispensed with.

[0022] This effect is due to the fact that the openings of the porous collector foil provide a larger contact surface between the electrode film or the electrode mixture and the porous collector foil than a non-porous collector foil (also called "solid foil"). In this way, a mechanical interlock or anchor is formed between the electrode film and the collector foil. In addition, due to the larger surface area of ​​the porous collector foil, the adhesion between the participating components is also increased.

[0023] In this case, sufficient contact and reliable adhesion between the electrode film and the porous collector foil is established by pressing the self-supporting electrode film and / or the dry electrode mixture.

[0024] In particular, the electrode film can be pressed at least partially through the openings in the porous collector foil so that even if a self-supporting electrode film is applied only on one side of the porous collector foil, a composite electrode is obtained in which the electrode film is present on both sides of the porous collector foil.

[0025] Preferably, the pressing is performed by calendering, in particular by cold calendering.

[0026] Calendering allows for a particularly controlled process control, in which uniform forces are provided for pressing the electrode film.

[0027] “Cold calendering” is understood to mean that calendering is carried out at a temperature in the range of 10° C. to 60° C., in particular 10° C. to 50° C., preferably 15° C. to 30° C., for example at room temperature. In this way, the costs for generating higher temperatures can be saved and deformations due to temperature differences can be avoided or at least reduced.

[0028] The openings in the porous collector foil make the porous collector foil more flexible or elastic than a collector foil without corresponding openings. As a result, the porous collector foil has lower material stress and less warping during calendering, so that the produced electrode has a uniform shape, i.e. no warping or at least reduced warping, even when high forces are used during the calendering step. As a result, fewer ripples, wrinkles, cracks and cambers are also produced.

[0029] “Curvature” here means the deviation from rectilinearity after calendering, ie the deviation from a uniform profile with longitudinal sides oriented essentially parallel to one another.

[0030] Compared to continuous collector foils, such as rolled foils, porous collector foils also have the advantage of reduced weight. Porous collector foils are known from lightweight structures, are available worldwide and are easy to process.

[0031] The porous current collector foil is in particular a perforated foil, a punched foil, a cut foil, an etched foil, a slotted foil, a metal expanded metal or a metallized fabric.

[0032] Such a porous collector foil can be produced in a simple manner from a continuous collector foil, for example a rolled foil, a so-called “solid foil”, and can be provided at low cost.

[0033] The porous current collector foil may be a metal expanded metal, which ensures good mechanical interlocking or anchoring between the electrode membrane and the porous current collector foil due to its large surface area.

[0034] The metallized fabric has a particularly high flexibility and a low dead weight. In this way, the energy density of an electrochemical cell having a composite electrode produced according to the invention can be further increased.

[0035] For example, DE 10 2018 000 272 A1 describes metallized glass fabrics as collectors in lithium-ion cells.

[0036] In order to further improve the interaction between the electrode film and the porous collector foil, the porous collector foil can be cleaned and / or surface activated before applying the self-supporting electrode film. In this way, impurities such as process oil on the collector foil can be removed.

[0037] Particularly good cleaning results can be achieved by corona surface treatment.

[0038] Alternatively, the collector foil can also be pre-treated by means of plasma etching.

[0039] In principle, wet-chemical cleaning of the porous collector foil is also possible, for example pickling with sodium hydroxide solution. However, wet-chemical cleaning is less preferred in order to be able to carry out the method according to the invention with as few or as few wet-chemical steps as possible.

[0040] In one approach, a first self-supporting electrode film is applied to the upper side of a porous collector foil and a second self-supporting electrode film is applied to the lower side of the porous collector foil opposite to the upper side, both of which are pressed onto the porous collector foil.

[0041] In this way, the corresponding electrode films can be applied and fixed to both sides of the porous collector foil in a single method step, so that the overall time required for applying the electrode films can be further reduced.

[0042] Furthermore, during pressing, in addition to the interaction between the corresponding electrode membrane and the porous collector foil, an interaction also occurs between the two electrode membranes, which are loaded with pressure from the top and bottom, so that the interaction between the two pressed electrode membranes can ensure further mechanical stability of the manufactured composite electrode.

[0043] Furthermore, such a process can be carried out in the vertical direction of the collector foil, wherein the electrode film is pressed, for example, by means of calendering rollers arranged on both sides and opposite to each other.

[0044] The process is preferably carried out without solvents. In this way, the costs of the process can be further reduced and the use of ecologically harmful solvents such as NMP (N-methylpyrrolidone) can be avoided.

[0045] Furthermore, the object of the invention is achieved by a composite electrode for an electrochemical cell, which is obtainable by the above-described method.

[0046] In particular, the composite electrode is obtained according to the above method.

[0047] Composite electrodes can be produced particularly cost-effectively and have no or only little dead material.

[0048] Furthermore, the object of the invention is achieved by an electrochemical cell comprising at least one composite electrode of the type described above.

[0049] The electrochemical cell according to the invention has, in particular, a high energy density, since no additional coating containing an adhesion promoter is necessary.

[0050] In particular, all electrodes of the electrochemical cell are composite electrodes of the above-mentioned type.

[0051] The electrochemical cells are preferably lithium ion cells.

[0052] The term "lithium-ion cell" is used synonymously in the present context for all names commonly used in the prior art for lithium-containing primary cells and cells, such as lithium batteries, lithium cells, lithium polymer cells, lithium-ion battery cells and lithium-ion accumulators. In particular, this includes rechargeable batteries (secondary batteries). BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Further features and characteristics of the present invention are given by the following detailed description of exemplary embodiments, which are not to be considered restrictive, and by the accompanying drawings.

[0054] The attached pictures are as follows:

[0055] FIG. 1 shows a method for manufacturing an electrode as known in the prior art;

[0056] Figure 2 A schematic diagram showing a first embodiment of a composite electrode according to the invention as obtainable by means of the method according to the invention;

[0057] Figure 3 A schematic diagram showing a second embodiment of a composite electrode according to the present invention;

[0058] Figure 4 A schematic diagram showing a third embodiment of a composite electrode according to the present invention;

[0059] Figure 5 A method for producing an electrode, in particular according to Figures 2 to 4 A block diagram of the method of the present invention for a composite electrode;

[0060] Figure 6 Show Figure 5 A schematic diagram of multiple sub-steps of a first embodiment of the method of the present invention; and

[0061] Figure 7 Show Figure 5 Schematic diagram of a sub-step of the second embodiment of the method of the present invention. DETAILED DESCRIPTION

[0062] FIG. 1 schematically shows a method for producing an electrode as known in the prior art.

[0063] In this method, electrode films 12 are applied on both sides, ie both toward upper side 14 and toward lower side 16 of collector foil 10 opposite upper side 14 , to collector foil 10 , which is made of metal such as copper or aluminum, for example.

[0064] The electrode film 12 is pressed onto the upper side 14 or the lower side 16 by means of hot lamination, ie at a temperature of typically about 110° C. to 150° C. and with a predetermined pressure, as indicated by the arrows in FIG. 1 .

[0065] In order to provide adequate adhesion between the collector foil 10 and the electrode film 12 , a primer coating 18 containing an adhesion promoter is applied both to the upper side 14 and to the lower side 16 .

[0066] This adhesion promoter must be applied to the collector foil 10 in an upstream step and remains as dead material in the finished electrode.

[0067] Figure 2 A schematic cross-sectional view of a composite electrode 20 according to the invention is shown, which is obtained by a method according to the invention for producing an electrode, which method will be described in more detail below.

[0068] The composite electrode 20 includes a porous collector foil 22 including a plurality of openings 24 extending through the porous collector foil 22 .

[0069] In other words, the openings 24 extend from the upper side 26 of the porous collector foil 22 to the lower side 28 of the porous collector foil 22 .

[0070] Figure 2 24. It should be understood that the porous collector foil 22 has a cross-sectional view extending directly through the opening 24. Figure 2 The regions shown separately in the figure are connected to each other at other locations along the lateral extension direction of the porous collector foil 22.

[0071] The composite electrode 20 also includes a self-supporting electrode film 30 including a plurality of dry-processed particles including a binder, a conductive additive, and an active material.

[0072] The types of the binder, conductive additive, and active material are not further limited as long as a self-supporting electrode film can be prepared from them.

[0073] In particular, a self-supporting electrode membrane 30 is produced according to the method described in US 2013 / 0157141 A1. Dry, free-flowing particles containing active materials, binders and additives are mixed with one another and compacted, for example using a roller mill, to form a self-supporting, i.e. self-stable electrode membrane. In particular, a "fibrillable" polymer such as polytetrafluoroethylene (PFTE) is used as a binder.

[0074] In principle, instead of a self-supporting electrode membrane 30 , it is also possible to use a dry electrode mixture which can contain the same components as the self-supporting electrode membrane 30 described above.

[0075] According to the invention, the composite electrode 20 has no adhesion promoter, ie, is not provided with a coating similar to the primer coating 18 (see FIG. 1 ).

[0076] Instead, sufficient adhesion of the electrode film 30 on the porous collector foil 22 is ensured by the electrode film 30 extending through the openings 24 of the porous collector foil 22 in the composite electrode 20. At the same time, the electrode film 30 covers the upper side 26 and the lower side 28 of the porous collector foil 22 to a large extent.

[0077] In other words, with the outer dimensions unchanged, the contact surface between the porous collector foil 22 and the electrode film 30 is higher than the available contact surface between the current collector 10 (without openings) and the electrode film 12 in FIG. 1 .

[0078] In addition, the electrode film 30 is mechanically fixed to prevent slipping, warping or falling off, such as by Figure 2 As shown by the double-headed arrow in .

[0079] The composite electrode 20 according to the invention thus enables electrochemical cells with increased energy density, since the primer coating 18 which constitutes only dead material with respect to the maximum achievable energy density can be omitted without having to accept a loss in durability and mechanical load-bearing capacity of the composite electrode 20 .

[0080] The protruding regions of the porous collector foil 22 , ie the regions to which no electrode film 30 is applied, can later be used as collector tabs of the composite electrode 20 in the installed position.

[0081] There is no further limitation on the material of the porous collector foil 22. For example, the porous collector foil 22 is made of copper or aluminum.

[0082] In the first embodiment, the porous collector foil 22 is a perforated foil.

[0083] exist Figure 3 A second embodiment of the composite electrode 20 according to the present invention is shown in FIG.

[0084] The second embodiment corresponds substantially to the first embodiment, so that only the differences will be discussed below. The same reference numerals denote the same or functionally identical components and reference is made to the above description.

[0085] In a second embodiment, the porous collector foil 22 is a metal expanded metal.

[0086] Expanded metal is available worldwide at low cost and has a flexible mesh structure. In this way, a particularly advantageous mechanical interlock is achieved between the porous collector foil 22 and the electrode membrane 30 .

[0087] Expanded metal is known, for example, from lightweight construction.

[0088] A similar structure can also be realized with the aid of a porous collector foil 22 made of a metallized fabric.

[0089] exist Figure 4 A third embodiment of the composite electrode 20 according to the present invention is shown in FIG.

[0090] The third embodiment corresponds substantially to the first and second embodiments, so that only the differences are discussed below. The same reference numerals denote the same or functionally identical components and reference is made to the above description.

[0091] In a third embodiment, the porous collector foil 22 is a slotted foil, so that the openings 24 extend obliquely through the porous collector foil 22 from an upper side 26 to a lower side 28 .

[0092] The method according to the invention for producing an electrode for an electrochemical cell, ie a composite electrode as described above, is explained in detail below.

[0093] First, a self-supporting electrode film 30 and a porous collector foil 22 (see Figure 5 Steps S1 and S2).

[0094] Optionally, the porous collector foil 22 can be pretreated by cleaning and / or surface activation of the porous collector foil 22 , for example by means of a corona surface treatment.

[0095] Next, the self-supporting electrode film 30 is applied and pressed onto the porous collector foil 22 (see Figure 5 , step S3 in the above process).

[0096] exist Figure 6 Schematically illustrated are selected method steps of a first embodiment of the method according to the invention.

[0097] In this embodiment, the self-supporting electrode film 30 is applied to the upper side 26 of the porous collector foil 22 and subsequently pressed by means of a calendering roller 32 .

[0098] The electrode film 30 is pressed through the opening 24 by the pressure exerted by the calendering rollers and, after pressing, covers both the upper side 26 and the lower side 28 of the porous collector foil 22 .

[0099] Calendering is preferably carried out at a temperature in the range of 10° C. to 60° C., in particular 10° C. to 50° C., preferably 15° C. to 30° C., in particular at room temperature.

[0100] In principle, the electrode film 30 can also not be pressed completely through the opening 24, but only pressed to such an extent that sufficient adhesion is produced between the electrode film 30 and the porous collector foil 22. In this case, the second electrode film 30 is then applied and also pressed on the opposite side of the porous collector foil 22.

[0101] exist Figure 7 FIG. 2 schematically shows a step of pressing the electrode film 30 in a second embodiment of the method according to the present invention.

[0102] The second embodiment of the method according to the invention corresponds essentially to the first embodiment, so that only the differences are discussed below. Reference is made to the above description.

[0103] In the second embodiment, not only an electrode film 30 (hereinafter also referred to as the first electrode film) is applied to the upper side 26 of the porous collector foil 22, but also an electrode film 30 (hereinafter also referred to as the second electrode film) is applied to the lower side 28 of the porous collector foil 22, and pressed with the aid of two opposing calendering rollers 32 to obtain a composite electrode 20.

[0104] In this way, the top side 26 and the bottom side 28 can be coated simultaneously in a single method step, whereby the process time required for producing the composite electrode 20 can be reduced to a minimum.

[0105] In addition, the process can be carried out in vertical process control. In other words, the manufacturing process can be designed so that the composite electrode 20 is manufactured by moving against or along the vertical direction V. Figure 7 In FIG. 1 , the region of the composite electrode 20 which has not yet been pressed and is shown at the top is geodesically higher than the region of the composite electrode 20 which has already been pressed and is shown at the bottom.

[0106] An experimental example of the method of the present invention for manufacturing an electrode is described below using a cathode as an example.

[0107] 91% by weight of NMC 622 as active material, 5% by weight of PTFE as binder and 4% by weight of conductive carbon black (Super Black C65) (in each case relative to the total weight of all components) were mixed.

[0108] In this case, the PTFE-containing binder is dry fibrillated, ie, binder fibers are formed, which are intertwined with the other components of the mixture or bind them together (as described in US 2013 / 00157141 A1). The mixture is calendered and a weight per unit area of ​​36 mg / cm is obtained. 2 And the electrode density is 3.4 g / cm 3 A self-supporting cathode film.

[0109] The self-supporting cathode film produced in this way was calendered at room temperature onto an aluminum expanded metal (having a thickness of approximately 38 μm) serving as a porous current collector foil, wherein after calendering, the expanded metal collector was completely surrounded by the cathode film.

Claims

1. A method for producing an electrode for an electrochemical cell, the method comprising the following steps: - providing a self-supporting electrode film (30) and / or a dry electrode mixture, the self-supporting electrode film and / or the dry electrode mixture comprising a plurality of dry-processed particles, the plurality of dry-processed particles comprising at least one binder, a conductive additive and an active material; - providing a porous collector foil (22) having openings (24) extending through the porous collector foil (22); and - applying and pressing a self-supporting electrode film (30) and / or a dry electrode mixture onto a porous collector foil (22) to form a composite electrode (20), wherein the electrode film (30) or the dry electrode mixture is at least partially pressed into the openings (24) of the porous collector foil (22), and the composite electrode (30) does not contain an adhesion promoter.

2. The method according to claim 1, wherein: The pressing is performed by calendering.

3. The method according to claim 2, wherein: The pressing is performed by cold calendering at a temperature in the range of 10°C to 60°C.

4. A method according to any one of the preceding claims, wherein: The porous collector foil (22) is a perforated foil, a cut foil, an etched foil, a punched foil, a slotted foil, a metal plate mesh or a metallized fabric.

5. A method according to any one of the preceding claims, wherein: The porous collector foil (22) is cleaned and / or surface activated before the self-supporting electrode film (30) is applied.

6. A method according to any one of the preceding claims, wherein: The porous collector foil (22) is pre-treated by corona treatment or plasma etching.

7. A method according to any one of the preceding claims, wherein: A first self-supporting electrode film (30) is applied to an upper side (26) of a porous collector foil (22) and a second self-supporting electrode film (30) is applied to a lower side (28) of the porous collector foil (22) opposite to the upper side (26), wherein both the first self-supporting electrode film (30) and the second self-supporting electrode film (30) are pressed onto the porous collector foil (22).

8. A method according to any one of the preceding claims, wherein: The process is carried out in the absence of solvent.

9. Composite electrode for electrochemical cells, obtainable by the method according to any one of the preceding claims.

10. Electrochemical cell comprising at least one composite electrode (20) according to claim 9.

Citation Information

Cited By

  • Dry electrode, secondary battery, and dry electrode manufacturing method

    WO2026172554A1