Preparation method of bismuth-based composite photocatalyst for regulating and controlling heterogeneous oxide
The bismuth-based composite photocatalyst is prepared by using a halide molten salt one-step modification method in the photocatalyst to form a nanosheet stacking structure, which solves the problems of complex morphology and modification process of existing photocatalysts, and improves catalytic activity and product purity. , suitable for industrial production.
Patent Information
- Application Number
- CN202410828539.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-25
AI Technical Summary
The morphology of existing photocatalysts is mostly thick sheets with small surface area and few active sites, which limits the pollutant degradation efficiency. Moreover, the modification process of composite heterogeneous catalytic materials is complicated and there are problems with impurity crystal phases.
Molten halide salt is used as the reaction medium, and a bismuth-based composite photocatalyst is prepared through a one-step modification method to form a nanosheet stack structure to increase active sites. The band gap position is controlled by controlling the halogen concentration to simplify the process.
It improves the light utilization rate and catalytic activity of the photocatalyst, reduces the calcination temperature, avoids the formation of impurity crystal phases, improves the purity and reaction efficiency of the product, simplifies the process flow, and is suitable for industrial production.
Smart Images

Figure CN118744000A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysts, and particularly relates to a method for preparing a bismuth-based composite photocatalyst for regulating multiphase oxides. Background Art
[0002] In the field of pollution treatment, photocatalytic technology can use solar energy to degrade pollutants in dye wastewater into inorganic small molecules, which is a means to solve pollution. By separately calcining various oxides Bi2O3, SiO2, and WO3, and obtaining the required crystal phase through one-step modification, oxygen vacancies are generated on the surface of the final bismuth silicate-bismuth tungstate heterostructure, which can produce more active groups. This method can also control the halogen concentration to regulate the band gap position and obtain a smaller band gap.
[0003] Currently, whether it is a single-component photocatalyst or a composite heterogeneous catalytic material, its morphology mostly presents a thick flake-like accumulation, the surface area cannot be restricted, and the active sites cannot be effectively exposed, further limiting the degradation efficiency of pollutants. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing a bismuth-based composite photocatalyst with regulated multiphase oxides. The method has a simple process, simple equipment requirements, and adjustable reaction conditions. The prepared material has high purity and good crystallinity. The obtained composite photocatalyst has a uniform particle size distribution, a nanosheet stacking structure, and more active sites. This structure can effectively improve the utilization rate of light and improve the photocatalytic activity.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides comprises the following steps:
[0007] Step 1, mixing bismuth silicate (Bi2SiO5) powder, bismuth tungstate powder and the first part of halide molten salt, and mixing by ball milling to obtain bismuth silicate-bismuth tungstate composite powder;
[0008] Step 2: Perform one of the following methods:
[0009] Method 1: The bismuth silicate-bismuth tungstate composite powder is washed alternately with deionized water and ethanol for several times to wash away the residual salt in the product, the washed powder is dried, reacted in a water bath, and the pH value is adjusted to 1-2, and a second part of the halide molten salt is added to continue the reaction. After drying and washing, the modified powder is obtained, that is, the composite photocatalyst prepared by the two-step method of bismuth tungstate-bismuth silicate-bismuth oxyhalide.
[0010] Method 2: The bismuth silicate-bismuth tungstate composite powder obtained in step 1 is not washed, the residual salt in the product is retained, a water bath reaction is carried out, and the pH value is adjusted to 1-2. After drying and washing, a modified powder is obtained, i.e., a composite photocatalyst prepared by one-step modification of bismuth tungstate-bismuth silicate-bismuth oxyhalide.
[0011] In one embodiment, the bismuth silicate powder is prepared by the following method:
[0012] Bi2O3 and SiO2 are used as reactants, NaCl and KCl are used as the third part of the halide molten salt, the reactants and the third part of the halide molten salt are loaded into a nylon jar, zirconium oxide is used as a grinding ball, mixed and ball-milled, heated to 500°C to 700°C at a heating rate of 10°C / min to 20°C / min in an air atmosphere, and then calcined for 4h to 7h to obtain bismuth silicate powder.
[0013] In one embodiment, the molar ratio of Bi2O3 to SiO2 is 1:1 to 1:9, the molar ratio of NaCl to KCl in the third part of the halide molten salt is 1:1, the mass percentage of the third part of the halide molten salt is 30% to 40%, and the ball milling time is controlled at 3 to 6 hours.
[0014] In one embodiment, the bismuth tungstate powder is prepared by the following method:
[0015] Take Bi2O3 and WO3 as reactants, NaCl and KCl as the fourth part of halide molten salt, grind Bi2O3 first, then add WO3 into Bi2O3 and mix and grind evenly, put the reactants and the fourth part of halide molten salt into a nylon jar, use zirconium oxide as grinding ball, mix and ball mill, heat to 630-660°C at a heating rate of 5°C / min in air atmosphere, and then calcine for 1-3h to obtain bismuth tungstate powder.
[0016] In one embodiment, the molar ratio of Bi2O3 to WO3 is 1:3; the molar ratio of NaCl to KCl in the fourth part of the halide molten salt is 1:1; the mass percentage of the fourth part of the halide molten salt is 30%, and the ball milling time is controlled at 3 to 6 hours.
[0017] In one embodiment, in the method 1, the temperature of the water bath reaction is 30° C., the time is 30 to 60 minutes, and the reaction is continued for 30 to 60 minutes after the pH is adjusted, and then the first part of the halide molten salt is added to continue the reaction for 2 to 3 hours.
[0018] In one embodiment, the first part of the halide molten salt is NaCl and / or KCl, accounting for 30% by mass.
[0019] In one embodiment, in the method 2, the temperature of the water bath reaction is 30°C to 50°C, the time is 30 to 60 minutes, and the reaction is continued for 30 to 60 minutes after the pH is adjusted.
[0020] In one embodiment, in the method 1 and the method 2, the drying and washing method is: washing with deionized water and ethanol alternately for several times, and drying in an oven at 60°C.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. This method uses halide molten salt as a reaction medium, which effectively reduces the calcination temperature. The halide molten salt medium helps to increase the reaction rate and product formation. In this method, Bi2O3, SiO2, WO3, and the subsequently generated bismuth tungstate and bismuth silicate can be evenly dispersed in the halide molten salt for reaction, and then directly modified in a water bath process, which solves the problem of impurity crystal phases in the product when a heterojunction is formed during the two-step modification process. Uniform mixing helps to improve the reaction efficiency and product purity.
[0023] 2. This scheme calcined different oxides Bi2O 3、 SiO 2、 WO3 and then the products are mixed for reaction, which promotes the breaking of bismuth oxygen bonds, thereby increasing the concentration of oxygen vacancies and promoting the generation of catalytic active groups; by controlling the concentration of different halogens, the generation of the desired crystalline phase is controlled. After one-step modification, it is easier to obtain adsorbed oxygen and bond breaking, which is beneficial to the improvement of the catalytic performance of the photocatalyst; through the one-step modification and control of the molten salt concentration by this method, the band gap position can be better regulated, and the composite bismuth silicate-bismuth tungstate heterogeneous photocatalyst produced by this method has a smaller band gap.
[0024] 3. The solid phase method for preparing bismuth silicate and bismuth tungstate is prone to form large-scale stacked morphology, with a small specific surface area and few active sites, which is not conducive to the photocatalytic process. This method improves the morphology of the composite photocatalyst by combining the halide molten salt method with a one-step liquid phase halogen modification. The bismuth tungstate photocatalyst modified with bismuth silicate is prone to form a nanosheet stacking structure, which can further promote the recombination between bismuth silicate and bismuth tungstate, thereby more efficiently forming a heterojunction, avoiding the formation of invalid heterostructures between the morphologies caused by thick sheet accumulation, reducing the recombination rate of photogenerated electrons and holes while improving the utilization rate of sunlight, so that the photocatalytic performance of the composite material is further improved.
[0025] 4. This method omits the washing step and directly obtains the bismuth silicate-bismuth tungstate composite photocatalyst material through water bath reaction modification, which simplifies the modification steps. The desired product structure and performance can be adjusted by regulating the reaction temperature and time. The reaction steps are simple and the reaction conditions are suitable, which is conducive to expanding the production scale and industrialization. At the same time, the product obtained by one-step modification has good ability to degrade organic dyes and some antibiotics, and the degradation effect is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a photocatalytic degradation curve of Rhodamine B degraded by a bismuth-based composite photocatalyst. DETAILED DESCRIPTION
[0027] The following is a detailed description of the implementation of the present invention in conjunction with the accompanying drawings and examples. The technical solution of the present invention is not limited to the specific implementations listed below, but also includes any combination of the specific methods.
[0028] A method for preparing a bismuth-based composite photocatalyst for regulating multiphase oxides, using bismuth silicate and bismuth tungstate as raw materials, and preparing a modified bismuth silicate heterogeneous photocatalytic material by one step. Based on the solid-phase method for preparing bismuth silicate and bismuth tungstate, the two are calcined separately and then mixed, and then modified and halogenated in one step by heating in a water bath to prepare a composite photocatalyst with a nanosheet stacking morphology. Specifically, the following steps are included:
[0029] Step 1, weigh Bi2O3 and SiO2 according to a certain molar ratio. Select NaCl and KCl as the third part of the halide molten salt used in the experiment to carry out the experiment, put the reactants and the third part of the halide molten salt into nylon cans respectively, use zirconium oxide as a grinding ball, mix and ball mill, and calcine at a certain temperature to obtain bismuth silicate (Bi2SiO5) powder.
[0030] Specifically, in this step, Bi2O3 and SiO2 in a molar ratio of 1:1, 1:3, or 1:9 can be mixed, and NaCl and KCl in a molar ratio of 1:1 to 1:3 can be added and mixed, and the two can be ball-milled for 3 to 5 hours. The obtained powder is calcined at 600 to 690° C. for 4 to 7 hours to obtain bismuth silicate (Bi2SiO5) powder. This step realizes the solid phase method for preparing bismuth silicate.
[0031] Step 2, weigh Bi2O3 and WO3 in molar ratio, select NaCl and KCl as the fourth part of the halide molten salt used in the experiment, grind the weighed Bi2O3 first, and then add the weighed WO3 to Bi2O3 and mix and grind evenly. The reactants and the fourth part of the halide molten salt are respectively put into nylon cans, mixed and ball-milled with zirconium oxide as grinding balls, and then calcined at a certain temperature to obtain bismuth tungstate powder.
[0032] Specifically, in this step, Bi2O3 and WO3 can be weighed in a molar ratio of 1:2 and 1:3, respectively, the weighed Bi2O3 is ground first, and then the weighed WO3 is added to Bi2O3 in 3 to 5 times for mixing and grinding. The reactants and the fourth part of the halide molten salt are respectively put into nylon tanks, and zirconium oxide is used as a grinding ball, mixed and ball-milled for 3 to 5 hours, and then calcined at 600 to 690°C to obtain bismuth tungstate powder; this step realizes the solid phase method for preparing bismuth tungstate.
[0033] Step 3, the product prepared in the above experiment is mixed with the first part of the halide molten salt in different ratios of bismuth silicate and bismuth tungstate, and ball milled for about 1 to 3 hours to mix the mixed powder evenly for subsequent reaction.
[0034] Step 4, wash the powder obtained in step 3 with deionized water and ethanol alternately for 3 to 6 times to wash away the residual salt in the product. After drying the washed powder, stir the reaction in a water bath at 30°C for 30 minutes, add nitric acid to adjust the pH value to 1, continue stirring for 30 to 60 minutes, and add the second part of the halide molten salt of different concentrations and types and stir for 2 to 3 hours. After drying and washing, the modified powder is obtained, that is, the composite photocatalyst prepared by the two-step method of bismuth tungstate-bismuth silicate-bismuth oxyhalide.
[0035] Step 5: The powder obtained in step 3 is not washed, reacted and stirred in a water bath at 30°C for 30 minutes, nitric acid is added to adjust the pH value to 1, and stirring is continued for 30 to 60 minutes, and stirring is continued for 2 to 3 hours without adding halide molten salt. After drying and washing, the modified powder is obtained, that is, the composite photocatalyst prepared by one-step modification of bismuth tungstate-bismuth silicate-bismuth oxyhalide.
[0036] The catalyst has a nanosheet stacking structure and can be used to degrade organic dyes, antibiotics, etc.
[0037] The present invention uses halide molten salt as a reaction medium, effectively reduces the calcination temperature, increases the active sites of bismuth silicate and bismuth tungstate, and the one-step modification of the composite photocatalyst has no side reactions, avoiding the problems of heterogeneous phases and interfaces in multi-step modification. The bismuth-based composite photocatalyst is easy to form a nanosheet stacking morphology, can form a heterojunction more efficiently, reduce the recombination rate of photogenerated electrons-holes, and improve the utilization rate of sunlight, and the photocatalytic performance is further improved. The method has simple process, short cycle, simple equipment, low cost, and is conducive to industrialization. The obtained composite material has many active sites in the powder, exhibits high photocatalytic performance, and has good ability to degrade organic dyes and some antibiotics.
[0038] Several embodiments of the present invention are as follows.
[0039] Example 1
[0040] (1) Bi2O3 and SiO2 were weighed in a molar ratio of 1:3. NaCl and KCl were selected as the third part of the halide molten salt for the experiment. The molar ratio of NaCl and KCl was 1:1. The reactants and the third part of the halide molten salt were respectively placed in nylon jars, mixed and ball-milled for 3 hours using zirconium oxide as a grinding ball, and calcined at 630°C to obtain bismuth silicate powder.
[0041] (2) Bi2O3 and WO3 were weighed in a molar ratio of 1:3, and NaCl and KCl were selected as the fourth part of the halide molten salt for the experiment. The molar ratio of NaCl and KCl was 1:1. The weighed Bi2O3 was first ground, and then the weighed WO3 was added to Bi2O3 in 3 times and mixed and ground evenly. The reactants and the fourth part of the halide molten salt were respectively placed in nylon jars, mixed and ball-milled for 5 hours using zirconium oxide as a grinding ball, and then calcined at 630°C to obtain bismuth tungstate powder.
[0042] (3) The product prepared in the above experiment is mixed with the first part of the halide molten salt in different ratios of bismuth silicate and bismuth tungstate, and ball-milled for 2 hours to mix the above mixed powders evenly to obtain a bismuth silicate-bismuth tungstate heterogeneous photocatalyst, that is, the photocatalyst with the nanosheet stacking structure morphology.
[0043] (4) The bismuth silicate-bismuth tungstate powder obtained in (3) was washed 4 times with deionized water and ethanol alternately to remove the residual salt in the product. The washed powder was dried, stirred in a water bath at 30° C. for 30 minutes, nitric acid was added to adjust the pH value to 1, and stirring was continued for 30 minutes. The second part of the halide molten salt of different concentrations was added and stirred for 2 hours. After drying and washing, the modified powder was obtained.
[0044] (5) The bismuth silicate-bismuth tungstate powder obtained in (3) was stirred in a water bath at 30° C. for 30 minutes without washing, nitric acid was added to adjust the pH value to 1, and stirring was continued for 30 minutes. The molten salt of halide was not added and stirring was continued for 2 hours. After drying and washing, the modified powder was obtained.
[0045] Example 2
[0046] (1) Bi2O3 and SiO2 were weighed in a molar ratio of 1:9. NaCl and KCl were selected as the third part of the halide molten salt for the experiment, and the molar ratio of NaCl and KCl was 1:1. The reactants and the third part of the halide molten salt were respectively placed in nylon jars, mixed and ball-milled for 3 hours using zirconium oxide as a grinding ball, and calcined at 660°C to obtain bismuth silicate powder.
[0047] (2) Bi2O3 and WO3 were weighed in a molar ratio of 1:3, and NaCl and KCl were selected as the fourth part of the halide molten salt for the experiment. The molar ratio of NaCl and KCl was 1:1. The weighed Bi2O3 was first ground, and then the weighed WO3 was added to Bi2O3 in 4 times and mixed and ground evenly. The reactants and NaCl and KCl were selected as the fourth part of the halide molten salt for the experiment. The molar ratio of NaCl and KCl was 1:1. The halide molten salt was respectively loaded into nylon jars, mixed and ball-milled for 5 hours using zirconium oxide as grinding balls, and then calcined at 660°C to obtain bismuth tungstate powder;
[0048] (3) The product prepared in the above experiment is mixed with the first part of the halide molten salt in different ratios of bismuth silicate and bismuth tungstate, and ball milled for 2 hours to mix the above mixed powders evenly to obtain bismuth silicate-bismuth tungstate heterogeneous photocatalyst, that is, the structural morphology photocatalyst.
[0049] (4) The bismuth silicate-bismuth tungstate powder obtained in (3) was washed 4 times with deionized water and ethanol alternately to remove the residual salt in the product. The washed powder was dried, stirred in a water bath at 30° C. for 40 minutes, nitric acid was added to adjust the pH value to 1, and stirring was continued for 30 minutes. The second part of the halide molten salt of different concentrations was added and stirred for 3 hours. After drying and washing, the modified powder was obtained.
[0050] (5) The bismuth silicate-bismuth tungstate powder obtained in (3) was stirred in a water bath at 30° C. for 40 minutes without washing, nitric acid was added to adjust the pH value to 1, stirring was continued for 30 minutes, and stirring was continued for 3 hours without adding halide molten salt. After drying and washing, the modified powder was obtained.
[0051] Figure 1 The photocatalytic degradation curve of the catalyst obtained in this example is put into a solution containing Rhodamine B organic dye and degraded. In the experiment, 30 mL of Rhodamine B was taken, wherein the concentration of Rhodamine B was 10 mg / L, and the amount of catalyst added was 3 mg. After the addition, the photocatalytic reaction was carried out for 180 min, wherein the dark reaction was 60 min and the light reaction was 120 min. It can be seen that under the condition of 120 min of illumination, the degradation rate was close to 100%.
[0052] In more embodiments of the present invention, the aforementioned parameters are combined in different types. For example, in step 1), the molar ratios of Bi2O3 and SiO2 are selected as 1:1, 1:3, 1:9, and 1:12, respectively, and the calcination temperatures are selected as 600°C, 630°C, 660°C, and 690°C, respectively. The results show that bismuth silicate powder can be prepared.
[0053] Similarly, in step 2), the heating rates were 10°C / min, 15°C / min, and 20°C / min, and the calcination temperatures were 600°C, 630°C, 660°C, and 690°C. The results showed that bismuth tungstate powders could be prepared.
[0054] Similarly, during the ball milling mixing in step 3), the ball milling time is selected to be 1 hour, 2 hours, and 3 hours. The results show that bismuth silicate-bismuth tungstate heterogeneous photocatalyst can be prepared.
[0055] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, substitutions, combinations, simplifications, etc. made based on the principles or spirit of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides, characterized in that: The steps include: Step 1, mixing bismuth silicate powder, bismuth tungstate powder and the first part of halide molten salt, and mixing by ball milling to obtain bismuth silicate-bismuth tungstate composite powder; Step 2: Perform one of the following methods: Method 1: The bismuth silicate-bismuth tungstate composite powder is washed alternately with deionized water and ethanol for several times to wash away the residual salt in the product, the washed powder is dried, reacted in a water bath, and the pH value is adjusted to 1-2, and a second part of the halide molten salt is added to continue the reaction. After drying and washing, the modified powder is obtained, that is, the composite photocatalyst prepared by the two-step method of bismuth tungstate-bismuth silicate-bismuth oxyhalide. Method 2: The bismuth silicate-bismuth tungstate composite powder obtained in step 1 is not washed, the residual salt in the product is retained, a water bath reaction is carried out, and the pH value is adjusted to 1-2. After drying and washing, a modified powder is obtained, i.e., a composite photocatalyst prepared by one-step modification of bismuth tungstate-bismuth silicate-bismuth oxyhalide.
2. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1, characterized in that: The bismuth silicate powder is prepared by the following method: Bi2O3 and SiO2 are used as reactants, NaCl and KCl are used as the third part of the halide molten salt, the reactants and the third part of the halide molten salt are loaded into a nylon jar, zirconium oxide is used as a grinding ball, mixed and ball-milled, heated to 500°C to 700°C at a heating rate of 10°C / min to 20°C / min in an air atmosphere, and then calcined for 4h to 7h to obtain bismuth silicate powder.
3. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 2, characterized in that: The molar ratio of Bi2O3 to SiO2 is 1:1-1:9, the molar ratio of NaCl to KCl in the third part of the halide molten salt is 1:1, the mass percentage of the third part of the halide molten salt is 30%-40%, and the ball milling time is controlled at 3-6 hours.
4. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1, characterized in that: The bismuth tungstate powder is prepared by the following method: Take Bi2O3 and WO3 as reactants, NaCl and KCl as the fourth part of halide molten salt, grind Bi2O3 first, then add WO3 into Bi2O3 and mix and grind evenly, put the reactants and the fourth part of halide molten salt into a nylon jar, use zirconium oxide as grinding ball, mix and ball mill, heat to 630-660°C at a heating rate of 5°C / min in air atmosphere, and then calcine for 1-3h to obtain bismuth tungstate powder.
5. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 4, characterized in that: The molar ratio of Bi2O3 to WO3 is 1:3; the molar ratio of NaCl to KCl in the fourth part of the halide molten salt is 1:1; the mass percentage of the fourth part of the halide molten salt is 30%, and the ball milling time is controlled at 3 to 6 hours.
6. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1, characterized in that: In the method 1, the temperature of the water bath reaction is 30° C., the time is 30 to 60 minutes, and the reaction is continued for 30 to 60 minutes after the pH is adjusted, and then the first part of the halide molten salt is added to continue the reaction for 2 to 3 hours.
7. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1 or 6, characterized in that: The first part of the halide molten salt is NaCl and / or KCl, accounting for 30% by mass.
8. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1, characterized in that: In the second method, the temperature of the water bath reaction is 30° C. to 50° C., the time is 30 to 60 minutes, and the reaction is continued for 30 to 60 minutes after the pH is adjusted.
9. The method for preparing a bismuth-based composite photocatalyst for regulating heterogeneous oxides according to claim 1, characterized in that: In the method 1 and the method 2, the drying and washing method is: washing with deionized water and ethanol alternately for several times, and drying in an oven at 60°C.
10. Use of the catalyst obtained by the preparation method of the bismuth-based composite photocatalyst for regulating heterogeneous oxides according to any one of claims 1 to 9 in degrading organic dyes and antibiotics.
Citation Information
Patent Citations
Preparation method of bismuth silicate powder
CN102351202A
In-situ growth interface adjustable multi-heterostructure photocatalyst and preparation method thereof
CN116099558A
Bismuth oxyhalide coated single crystal ternary positive electrode material and preparation method thereof
CN116487583A
Bi-guided controllable flower-like heterogeneous photocatalyst and preparation method thereof
CN117085715A
Bismuth oxyhalide compounds useful as photocatalysts
US20130334145A1