Welding method for NM400 wear-resistant steel with thickness of 20-40 mm

By using 80% Ar+20% CO2 mixed gas and HS-70 welding wire in wear-resistant steel welding, combined with welding groove design and preheating treatment, the problem of insufficient weld strength and impact toughness is solved, and high-quality NM400 wear-resistant steel welding effect.

CN118744265AInactive Publication Date: 2024-10-08BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410717726.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

While existing wear-resistant steel welding methods ensure structural safety and welded joint design performance, the weld strength and impact toughness are insufficient, and the process is complex and difficult to promote.

Method used

Use 80% Ar+20% CO2 mixed gas and HS-70 welding wire for welding. The welding groove is designed as a symmetrical double-sided X-shaped groove. Preheating before welding is 50-150°C. The welding current is 250-270A and the voltage is 25-30V. , speed 5-5.5mm/s, gas flow 15-20L/min, and polish and preheat the steel plate.

Benefits of technology

High-quality welding of 20-40mm thick NM400 wear-resistant steel plate welded joints has been achieved. The tensile strength of the weld is 850-880MPa, the impact energy is greater than 140J, the heat-affected zone is greater than 160J, and the welding quality and performance are excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744265A_ABST
    Figure CN118744265A_ABST
Patent Text Reader

Abstract

The invention discloses a welding method for NM400 wear-resistant steel with the thickness of 20-40 mm. An NM400 wear-resistant steel plate with the thickness of 20-40 mm is adopted, and a mixed gas of 80% of Ar and 20% of CO2 and an HS-70 welding wire are adopted for welding; a symmetrical double-sided X-shaped groove is adopted as a welding groove, the angle of a single-sided groove is 30 degrees, a truncated edge is 2 mm, and a groove gap is 1-2 mm; a steel plate is preheated before welding, the preheating temperature ranges from 50 DEG C to 150 DEG C, the diameter of a welding wire is phi 1.2 mm, the welding current is controlled to range from 250 A to 270 A, the welding voltage is controlled to range from 25 V to 30 V, the welding speed is controlled to range from 5 mm / s to 5.5 mm / s, and the gas flow ranges from 15 L / min to 20 L / min. According to the welding method for the NM400 wear-resistant steel with the thickness of 20-40 mm, the welding quality of a connector is good, and the connector has excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant steel welding, in particular to a welding method for 20-40mm thick NM400 wear-resistant steel. Background Art

[0002] Wear-resistant steel has high strength, high hardness and high wear resistance, and is widely used in mining and various engineering machinery fields. The production process of wear-resistant steel uses high carbon and high alloy content, and the carbon equivalent is large, but it needs to be welded during use, so the welding formability of wear-resistant steel has also become the focus of users. When welding wear-resistant steel, it is necessary not only to ensure the safety and reliability of the structure, but also to require the comprehensive performance of the welded joint to meet the design requirements. Therefore, it is of great significance to study the welding method of wear-resistant steel.

[0003] Patent CN 114309899A discloses a welding method for low alloy wear-resistant steel and its welding joint. Double fine wire submerged arc welding is used for base and filling welding, and cold wire filling double fine wire submerged arc welding is used for cover to ensure the comprehensive mechanical properties of the weld. However, the weld strength is not provided in the invention, and the weld impact toughness is low. Patent CN 104227180B discloses a welding method for NM400 wear-resistant steel. First, A407 stainless steel electrode is used for base weld, then ER506 welding wire is used for multi-layer multi-pass welding, then A407 electrode is used to weld the transition layer, and finally D212 electrode is used for cover. The whole welding process uses a variety of welding materials and a variety of welding methods, and the welding process needs to be preheated at 350-400℃. The welding process is complicated and difficult to promote and implement. Summary of the invention

[0004] The purpose of the invention is to provide a 20-40 mm thick NM400 wear-resistant steel welding method, which has good joint welding quality and excellent performance.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention discloses a 20-40 mm thick NM400 wear-resistant steel welding method, which adopts a 20-40 mm thick NM400 wear-resistant steel plate, 80% Ar+20% CO2 mixed gas and HS-70 welding wire for welding;

[0007] The welding groove adopts a symmetrical double-sided X-shaped groove, with a single-sided groove angle of 30°, a blunt edge of 2mm, and a groove gap of 1-2mm;

[0008] The steel plate is preheated before welding, the preheating temperature is 50-150℃, the welding wire diameter is Φ1.2mm, the welding current is controlled at 250-270A, the welding voltage is controlled at 25-30V, the welding speed is controlled at 5-5.5mm / s, and the gas flow rate is 15-20L / min.

[0009] Furthermore, the wear-resistant steel plate is polished before welding to remove rust and oil stains within 20 mm around the weld.

[0010] Furthermore, the preheating temperature is 80-120°C.

[0011] Furthermore, the preheating temperature is 50°C, 100°C or 150°C.

[0012] Furthermore, the weld tensile strength is 850-880 MPa.

[0013] Furthermore, the impact energy of the weld at -20℃ is greater than 140J.

[0014] Furthermore, the heat affected zone is greater than 160J.

[0015] Compared with the prior art, the beneficial technical effects of the present invention are:

[0016] The invention adopts 20-40mm thick NM400 wear-resistant steel plate, 80% Ar+20% CO2 mixed gas and solid welding wire HS-70 argon-rich mixed gas shielded welding, the preheating temperature before welding is 50-150°C, the joint welding quality is good and has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention will be further described below in conjunction with the accompanying drawings.

[0018] Figure 1 The present invention discloses a macroscopic metallographic structure of a welded joint of a 20-40 mm thick NM400 wear-resistant steel plate. DETAILED DESCRIPTION

[0019] The invention provides a 20-40 mm thick NM400 wear-resistant steel welding method, which adopts 20-40 mm thick NM400 wear-resistant steel plates, 80% Ar+20% CO2 mixed gas and HS-70 welding wire for welding.

[0020] The welding groove adopts a symmetrical double-sided X-shaped groove, with a single-sided groove angle of 30°, a blunt edge of 2mm, and a groove gap of 1-2mm.

[0021] The steel plate is preheated before welding, the preheating temperature is 50-150℃, the welding wire diameter is Φ1.2mm, the welding current is controlled at 250-270A, the welding voltage is controlled at 25-30V, the welding speed is controlled at 5-5.5mm / s, and the gas flow rate is 15-20L / min.

[0022] After welding, the weld is subjected to non-destructive testing. After passing the inspection, the weld metal mechanical properties such as tensile strength, impact toughness, and bending of the joint are sampled and tested.

[0023] The present invention will be further described in detail below in conjunction with specific embodiments.

[0024] Examples 1 to 3 are the process steps adopted by the welding method of 20-40 mm thick NM400 wear-resistant steel plate of the present invention.

[0025] The welding process parameters of each embodiment and comparative example are shown in Table 1; the mechanical properties of the obtained welded joints are shown in Table 2.

[0026] Table 1 Welding process parameters

[0027]

[0028] Table 2 Welding joint properties

[0029]

[0030] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A welding method for 20-40mm thick NM400 wear-resistant steel, characterized in that: Use 20-40mm thick NM400 wear-resistant steel plate, 80% Ar + 20% CO2 mixed gas and HS-70 welding wire for welding; The welding groove adopts a symmetrical double-sided X-shaped groove, with a single-sided groove angle of 30°, a blunt edge of 2mm, and a groove gap of 1-2mm; The steel plate is preheated before welding, the preheating temperature is 50-150℃, the welding wire diameter is Φ1.2mm, the welding current is controlled at 250-270A, the welding voltage is controlled at 25-30V, the welding speed is controlled at 5-5.5mm / s, and the gas flow rate is 15-20L / min.

2. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: Before welding, grind the wear-resistant steel plate and remove rust and oil stains within 20mm around the weld.

3. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: The preheating temperature is 80-120℃.

4. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: The preheating temperature is 50°C, 100°C or 150°C.

5. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: The tensile strength of the weld is 850-880MPa.

6. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: The impact energy of the weld joint at -20℃ is greater than 140J.

7. The 20-40 mm thick NM400 wear-resistant steel welding method according to claim 1, characterized in that: The heat affected zone is greater than 160J.

Citation Information

Patent Citations

  • Argon-enriched mixed gas protection welding method for high-strength abrasion-resistant steel

    CN102049597A

  • Non-preheating gas shielded welding method for wear-resistant steel plate

    CN105149746A

  • Preheating-free efficient welding method suitable for wear-resistant steel plate

    CN113182648A

  • Argon-rich mixed gas shielded welding method for NM450 high-strength wear-resistant steel

    CN114178664A

  • Welding method for NM500 wear-resistant steel subjected to rare earth treatment

    CN115446497A