Preparation method of nitride nano micro powder

Using laser radiation to prepare nitride nanopowders in a normal pressure nitrogen environment through high-temperature gasification and combination reactions and recrystallization synthesis processes, it solves the problems of inaccurate particle size control, low purity and environmental pollution in the existing technology, and achieves Efficient, low-cost, pollution-free production of nano-scale micron powder.

CN118744970APending Publication Date: 2024-10-08GANSU NANOMICRO LEAD SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965015.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing nitride nanopowder preparation methods have problems such as imprecise particle size control, low purity, complex processes, low productivity, high cost and environmental pollution, making it difficult to meet the needs of high-performance materials.

Method used

It adopts the preparation process of high-temperature gasification, combination reaction, and recrystallization synthesis, and uses the high-density energy radiation of laser in a closed normal-pressure nitrogen environment to cause a chemical reaction between elemental metal or non-metal raw materials and nitrogen to generate nitride powder, which is then passed through Particle growth, quenching and shaping and multi-stage cooling processes achieve nano-scale, ultra-fine and ultra-purified micro powder production.

Benefits of technology

The production of high-purity, nanoscale, adjustable and uniform particle size nitride nanopowder is achieved, which reduces production costs and increases output. The process is pollution-free and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744970A_ABST
    Figure CN118744970A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano materials, and particularly relates to a preparation method of nitride nano micro powder. In order to solve the problems of inaccurate product particle size control, low purity, complex process, low productivity, high cost, environmental pollution and the like in the existing domestic and overseas nitride nano micro powder preparation method, the invention provides a novel preparation process for high-temperature gasification, combination reaction and recrystallization synthesis. The method comprises the following steps: selecting a high-purity raw material, carrying out laser radiation gasification and combination reaction, and then carrying out cooling condensation growth, shock cooling shaping, cooling and collecting processes to obtain the high-purity nitride nano micro powder. The method is pollution-free in production process, short in production period, high in efficiency, low in energy consumption, low in investment and high in yield, and can be used for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano materials, and in particular relates to a method for preparing nitride nano powder. Background Art

[0002] With the rapid development of nanotechnology, nanomaterials exhibit properties that are completely different from macroscopic materials due to their unique size effects, surface effects, and quantum effects. They have shown great application potential in the fields of materials science, energy, electronics, and chemical engineering, providing unlimited possibilities for the design and development of new materials.

[0003] For example, in the field of nitride nanomaterials: nano aluminum nitride is used in the manufacture of integrated circuit substrates, electronic devices, optical devices, radiators, high-temperature crucibles for the preparation of metal-based and polymer-based composite materials, and has excellent application prospects, especially in high-temperature sealing adhesives and electronic packaging materials to improve the heat dissipation performance and strength characteristics of materials. Nano titanium nitride is resistant to high temperatures, resistant to oxidation, and has high hardness. It has excellent infrared absorption and ultraviolet light shielding properties and good electrical conductivity. It can be used in thermal insulation coatings, automotive ceramic films, lead-free solder materials, green electronic materials, cemented carbide, high-temperature ceramic conductive materials, heat-resistant and wear-resistant materials, and other fields. Nano boron nitride has excellent physical and chemical properties and has good application prospects in the fields of transistor thermal desiccants, high thermal conductivity insulating coatings, insulating glues, thermal conductive films, high-temperature lubricants, release agents, atomic reactor structural materials, and other fields. Nano silicon nitride can be used to manufacture structural components in industries such as metallurgy, chemical industry, machinery, aviation, aerospace and energy, surface treatment of molds, cutting tools, turbine blades, turbine rotors, ceramic and graphite-based composite materials, rubber, plastics, coatings, adhesives and other polymer-based composite materials.

[0004] However, the existing preparation methods of nitride nanopowders often have defects such as inaccurate product particle size control, low purity, complex process, low production capacity, high cost, environmental pollution, etc., which are difficult to meet the growing demand for high-performance materials. The present invention is based on the principles of economy, practicality and industrial production, and develops a new preparation method of nitride nanopowder to achieve low-cost, high-yield, large-scale and pollution-free production, and produce nano-level ultra-fine and ultra-purified nanomaterials. Summary of the invention

[0005] In view of the problems of inaccurate product particle size control, low purity, complex process, low production capacity, high cost and environmental pollution in the current preparation methods of nitride nano-powders at home and abroad, the present invention proposes a new preparation process of high-temperature gasification and chemical reaction, and recrystallization synthesis. The preparation process can realize the production of high-purity, nano-level, adjustable particle size and uniform particle size nitride nano-powder materials. The average particle size of the produced nitride powder is nano-level D50 5-100nm, with the advantages of small investment, low production cost, high output and no pollution, and is suitable for large-scale production.

[0006] Technical solution:

[0007] The present invention provides a method for preparing nitride nano-powder, including a method for preparing metal nitride and non-metal nitride nano-powder. The preparation method is to use high-density energy radiation of laser in a closed nitrogen environment at normal pressure to rapidly gasify single metal or non-metal raw materials and react with nitrogen to generate nitrides, and then cool and condense into spherical or irregular crystal nucleus particles, and then produce nano-level powder materials through particle growth, quenching and shaping, cooling, and collection processes. The preparation method is completed by a set of equipment to complete the process flow.

[0008] The complete set of equipment used in this preparation method includes: a high-power laser, a gasification reactor, a particle growth furnace, a quencher, a water-air cooler, a dust collector, a nitrogen generator, a storage tank, a vacuum unit, and a monitoring system. The entire process is completed in a relatively closed airflow channel, starting from the preparation of nitrogen by the nitrogen generator, and along the flow direction of nitrogen, the gasification reactor, the particle growth furnace, the quencher, the water-air cooler, and the inner cavity of the dust collector are connected in sequence through pipelines to form the entire airflow channel. At the same time, a circulation pipeline is installed at the end of the airflow channel and connected to the outlet of the nitrogen generator to reflux the nitrogen for recycling.

[0009] In the above equipment, the storage tank is used to store metal or non-metal raw materials, and is equipped with a feeding device for pushing the raw materials to the gasification platform in the gasification reactor. The outlet of the nitrogen generator is connected to two branch pipes, one of which is connected to the storage tank for replenishing nitrogen to the storage tank; the other pipe is connected to a fan and an electric heater, and then connected to the gasification reactor to provide a nitrogen gas flow with controllable flow and temperature to the gasification reactor. The gasification reactor is equipped with an independent temperature control and cooling device. The particle growth furnace is equipped with a separate temperature control heat dissipation device and an adjustable damper for adjusting and controlling the air flow temperature and air flow rate. The vacuum unit is connected to the storage tank and the air flow channel respectively, and is used to pre-vacuum the storage tank and the air flow channel before the complete set of equipment is put into operation. The monitoring system is used to monitor, adjust and control the operating status, operating parameters and process parameters of the air flow in the furnace chamber of each equipment throughout the process.

[0010] The whole process includes the following steps:

[0011] Step (1): Select a single element metal or single element non-metal material in the form of granules or powder with high purity as a raw material.

[0012] Step (2): Load the above raw materials required for 1 to 2 shifts into the storage tank from the feeding port of the storage tank, close the feeding port to make the storage tank airtight, and push a portion of the raw materials onto the gasification platform in the gasification reactor through the feeding device.

[0013] Step (3): Start the monitoring system and vacuum unit. Under the action of the vacuum pump, remove the original oxygen and air in the storage tank and the air flow channel, and reduce the vacuum pressure to below 100Pa. After the vacuum is completed, close the vacuum pipeline valve and shut down the vacuum unit. Then start the nitrogen generator and blower to fill the storage tank and the air flow channel with nitrogen, so that the pressure in the storage tank and the air flow channel reaches normal pressure, that is, 1 atmosphere.

[0014] Step (4): Start the high-power laser, gasification reaction furnace and its temperature control and cooling device, particle growth furnace and its temperature control and heat dissipation device, quencher, water-air cooler, dust collector and other equipment in sequence to put the entire set of equipment into operation. Under the action of the fan, nitrogen circulates in the air flow channel and the circulation pipeline, and is replenished by the nitrogen generator. Optionally, for the preparation of nitride nanopowders with a melting point above 1000°C, the electric heater at the outlet of the nitrogen generator can be started at the same time to heat the nitrogen to 500°C to 800°C before entering the gasification furnace.

[0015] Step (5): In the gasification reactor, the laser light emitted by the high-power laser is directly applied to the raw materials on the gasification platform. The high-density energy radiation of the laser is used to rapidly heat up the metal or non-metal raw materials and gasify them, reacting with nitrogen to form nitrides. The nitrides are then rapidly cooled down by the temperature gradient to form spherical or irregular shaped nitride crystal nucleus particles suspended in the nitrogen. The nitrogen is also rapidly heated to form a high-temperature airflow.

[0016] Step (6): under the action of airflow, the crystal nucleus particles of the nitride enter the particle growth furnace along with the high-temperature airflow; the particle growth furnace is equipped with a temperature-controlled heat dissipation device and an adjustable air door for adjusting and controlling the airflow temperature and airflow velocity, so that the airflow temperature at the outlet of the particle growth furnace is not lower than the melting point temperature of the nitride, and the crystal nucleus particles of the nitride further collide and condense in the high-temperature airflow disturbance to grow particles; the size of the grown particles is affected by the cavity length of the particle growth furnace, the airflow temperature, and the airflow velocity of the particle growth furnace. By setting the cavity length of the particle growth furnace, and controlling the airflow temperature and airflow velocity by the temperature-controlled heat dissipation device and the adjustable air door, the collision growth time and particle size of the suspended particles are controlled, thereby achieving accurate particle size classification.

[0017] Step (7): The grown nitride particles flow rapidly into a quencher along with the air flow, and the quencher uses carbon dioxide as a low-temperature refrigerant. In the low-temperature environment, the nitride particles are rapidly cooled, and the temperature drops below the melting point of the nitride. The rapid temperature change causes the nitride particles to rapidly solidify and take shape, thereby generating solid micropowder.

[0018] Step (8): The solid micropowder then enters the water-air cooler along with the air flow. The water-air cooler uses a multi-stage cooling method of water cooling plus air cooling to reduce the temperature of the solid micropowder to below 160°C before entering the dust collector.

[0019] Step (9): Finally, the solid micropowder enters the dust collector along with the air flow and is collected by the dust collector to obtain high-purity nano-scale micropowder.

[0020] In the above steps, the raw material is any one of single metals and non-metals, including but not limited to: aluminum, copper, magnesium, nickel, lithium, tungsten, iron, calcium, chromium, zinc, titanium, zirconium, tin, cobalt, hafnium, gallium, strontium, bismuth, vanadium, molybdenum, tantalum, niobium, antimony, germanium, manganese and other metals, carbon, silicon, boron and other non-metals; the melting point temperature of the nitride, wherein:

[0021] The melting point of aluminum nitride is 2200℃; the melting point of copper nitride is 300℃; the melting point of magnesium nitride is 800℃; the melting point of tungsten nitride is 600℃; the melting point of calcium nitride is 1195℃; the melting point of chromium nitride is 1650℃; the melting point of titanium nitride is 2930℃; the melting point of zirconium nitride is 2980℃; the melting point of tin nitride is 120℃; the melting point of hafnium nitride is 3310℃; the melting point of gallium nitride is 1700℃; the melting point of vanadium nitride is 2320℃; the melting point of molybdenum nitride is 1750℃; the melting point of tantalum nitride is 3360℃; the melting point of strontium nitride is 1030℃; the melting point of niobium nitride is 2300℃; the melting point of antimony nitride is 292℃; the melting point of germanium nitride is 850℃; the melting point of silicon nitride is 1900℃; the melting point of boron nitride is 2700℃.

[0022] In the above complete set of equipment, according to the product precision requirements, the dust collector uses a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process combining these dust collectors, among which the electrostatic dust collector uses a single-stage or multi-stage electrostatic dust collector to achieve accurate classification and collection of micro-powder materials. The monitoring system is equipped with a monitoring platform, an early warning and alarm system, and various equipment monitoring subsystems, which are used to monitor, adjust and control the operating status, operating parameters and process parameters of the airflow in the furnace chamber of each equipment throughout the process.

[0023] In the above process flow, firstly, high-purity metal or non-metal raw materials are selected and stored in a sealed storage tank. When the outlet valve of the nitrogen generator is closed, the inner cavity of the air flow channel of each device is connected with the circulation pipeline to form a completely closed channel. In this way, the vacuum unit can perform vacuum pretreatment on the air flow channel and the storage tank to reduce the vacuum pressure to below 100Pa. Then, nitrogen is filled into the air flow channel and the storage tank through the nitrogen generator, and the air pressure reaches normal pressure, that is, 1 atmosphere, to form an oxygen-free, normal pressure, nitrogen-filled process atmosphere. For the very small amount of oxygen that still remains after the air flow channel is evacuated, a small amount of high-temperature oxidation reaction of the raw materials occurs at the beginning of the operation of the gasification reactor, which can quickly consume the remaining oxygen completely, so that a completely oxygen-free production environment can be quickly established without affecting normal production.

[0024] After other equipment is started, the entire closed airflow channel still maintains normal pressure or near normal pressure operation. When the airflow passes through the gasification reactor, the raw material undergoes a gasification reaction, and the nitrogen expands due to heat, and the air pressure will increase. After that, the airflow cools down when passing through the particle growth furnace, quencher, and wind and water cooler, and the air pressure will decrease accordingly. At this time, the monitoring system monitors the changes in the air pressure and temperature of the inner cavity of each device in real time, and adjusts the nitrogen generator gas supply volume, fan power, high-power laser radiation power, particle growth furnace damper, and adjusts the quencher and wind and water cooler temperature to keep the air pressure in the equipment cavity at normal pressure or slightly positive pressure, and stably maintain it within the range of 100KPa to 110KPa. The equipment cavity maintains normal pressure or slightly positive pressure operation, which is conducive to reducing the pressure difference between the equipment cavity and the outside atmosphere, effectively preventing air from leaking into the equipment seal, and ensuring the safe operation of the equipment.

[0025] In order to prevent misoperation or other accidents, an automatic pressure relief valve is installed on the air flow pipeline of the equipment, which will automatically release the pressure when the air pressure in the air flow channel exceeds 120KPa.

[0026] In the above process flow, metal or non-metal raw materials are pre-stored in storage tanks, which are continuously fed to the gasification reactor by a feeding device, and nitrogen is continuously added to the air flow channel in the inner cavity of the equipment by a nitrogen generator. The raw materials are continuously subjected to laser radiation gasification and chemical reaction, condensation growth, rapid cooling and shaping, cooling, and collection. The production process is a continuous and uninterrupted production process.

[0027] The above technical solution adopts laser radiation gasification method to produce high-quality nano-powder materials. In the gasification reactor, metal or non-metal raw materials are subjected to focused radiation of high-power, high-energy-density lasers, and quickly absorb a large amount of energy to undergo explosive gasification and then react with nitrogen to form nitrides, and then quickly cool down and condense in nitrogen to form nitride crystal nucleus particles, and then enter the particle growth furnace with the airflow for further condensation and growth. The particle growth furnace is equipped with a temperature-controlled heat dissipation device and an adjustable damper to adjust and control the airflow temperature and airflow velocity, and is monitored and controlled in real time by the monitoring system platform. During the particle growth process, by setting the particle growth furnace cavity length and controlling the particle growth process parameters such as growth temperature, temperature gradient, and airflow velocity by the monitoring system, it can ensure that the particles grow in an orderly manner under the temperature gradient, and affect the collision growth time and particle size of the suspended particles, so as to achieve accurate particle size classification. After being processed in the particle growth furnace, the grown particles enter the quencher for rapid cooling, the temperature drops below the melting point, and they are quickly solidified and shaped. Finally, after further cooling in a water-air cooler and collection in a dust collector, high-purity, high-quality ultrafine nano-scale micro-powder materials are obtained.

[0028] In a particle growth furnace, by increasing the temperature of the airflow in the particle growth furnace chamber, or reducing the temperature difference between the inlet and outlet airflows, the stability and uniformity of the particle condensation temperature can be maintained, the particles can be prevented from agglomerating, and the uniformity of the particle size can be improved. Secondly, appropriately reducing the design length of the particle growth furnace chamber, or increasing the airflow velocity, will shorten the collision growth residence time of the suspended particles in the furnace chamber, and generate ultrafine particles. However, if the furnace chamber is too short or the airflow velocity is too fast, the airflow cooling in the furnace chamber will be difficult to control, and the cooling effect of the subsequent equipment will be affected, increasing the cooling load of the subsequent equipment; on the contrary, lengthening the design length of the furnace chamber, or reducing the airflow velocity, will prolong the particle growth time, and generate particles with larger particle sizes, but reducing the airflow velocity (and the laser power needs to be reduced accordingly) will reduce the equipment productivity and affect the output.

[0029] In order to solve the above problems, make the whole production line more convenient for fine adjustment, produce ultrafine powder or larger particle size powder, ensure the stability of particle growth temperature control, and achieve the expected equipment productivity, two sets of particle growth furnaces with the same furnace cavity size can be set in parallel and connected between the gasification reaction furnace and the quencher. The design of the furnace cavity size of a single set of particle growth furnaces can meet the production of ultrafine powders, and are equipped with independent temperature control and heat dissipation devices and adjustable air doors. In this way, when only one set of particle growth furnaces is opened to participate in production operation, ultrafine powder can be produced when the airflow reaches the set flow rate Q and flow velocity V; when two sets of particle growth furnaces are opened at the same time to participate in production operation, due to the diversion effect, the airflow flow rate of a single set of particle growth furnaces is reduced to Q / 2, and the airflow velocity is reduced to V / 2, so that the collision growth residence time of suspended particles in the furnace cavity is doubled, thereby generating larger particle size powders, and the total flow rate of the two sets of particle growth furnaces is Q, which can also achieve the expected equipment productivity. In both cases, the air flow velocity in the furnace cavity can be further fine-tuned by adjusting the fan and the size of the adjustable damper in the furnace cavity to ensure stable operation of the equipment and accurate control of the operating process parameters and product particle size.

[0030] Among the equipment used in the above technical solution, except for the gasification reactor and the particle growth furnace which are special equipment, the rest of the equipment are conventional process equipment. Among them, the gasification reactor and the particle growth furnace equipment are required to have strong high temperature resistance. The solution is that, first, the gasification reactor and the particle growth furnace use refractory materials that can withstand ultra-high temperatures (>2300°C) in non-vacuum or non-inert atmospheres, such as zirconium boride and hafnium boride composite ultra-high temperature ceramic refractory materials with a refractory temperature of more than 3000°C; second, the gasification reactor and the particle growth furnace are equipped with their own independent temperature control cooling devices and temperature control heat dissipation devices, and the temperature of the furnace cavity wall is automatically monitored and controlled by the monitoring system and the temperature control cooling and heat dissipation devices, so that the temperature of the furnace cavity wall is kept below the refractory temperature; third, the inner diameter of the furnace cavity is appropriately increased to increase the temperature difference between the gasification area in the gasification reactor and the inner wall of its furnace cavity, and the temperature difference between the central high-temperature jet area in the particle growth furnace and the inner wall of its furnace cavity, so as to prevent the cavity material from being damaged by high temperature.

[0031] The above technical solution can produce high-purity, nano-scale, high-quality nitride nano-powder materials with adjustable particle size and uniform particle size, and the average particle size of the powder is D50 5-100nm.

[0032] In particular, it is pointed out that the above technical scheme adopts an anaerobic storage and feeding process in a closed storage tank, including pre-storing raw materials in the storage tank, pre-vacuuming the storage tank and then filling it with nitrogen, and continuously feeding the material by a feeding device, so that the raw material storage and feeding process are in an anaerobic environment, achieving safe and reliable continuous feeding capabilities, solving the problem of continuous feeding under anaerobic production conditions, and making continuous batch production and industrial production possible.

[0033] Secondly, this technical solution adopts a nitrogen preheating process, and the nitrogen is heated to 500℃ to 800℃ through an electric heater before entering the gasification reactor. First, it increases the temperature of the air flow in the gasification reactor, helps to improve the gasification efficiency of the laser irradiated raw materials, is beneficial to improve the equipment productivity, and saves the energy consumption of high-power lasers; second, it increases the temperature of the raw materials condensed into liquid particles after gasification and chemical reaction, to ensure the stability of subsequent high-temperature particle growth in the particle growth furnace.

[0034] In addition, as mentioned above, the technical solution specifically proposes a dual particle growth furnace parallel process, which can produce ultra-fine powder or larger particle size powder on a production line without reducing the equipment productivity, meet the precision requirements of different products, achieve fine adjustment and product precision classification, and do not need to transform the production line due to product precision, which is conducive to reducing equipment investment costs and product costs. The gasification reactor and particle growth furnace use independent temperature control cooling and heat dissipation processes to effectively protect the furnace cavity material from high temperature damage, extend the service life of the equipment, and keep the high-temperature airflow temperature in the particle growth furnace stable, adjustable and controllable, ensuring stable particle growth and fine particle size adjustment.

[0035] In summary, the above technical scheme proposes a feasible process scheme for preparing nitride nano-powder materials by laser gasification reaction method. The specific process measures include: vacuum pretreatment process, normal pressure and closed nitrogen environment production process, storage tank oxygen-free storage and feeding process, nitrogen preheating process, continuous and uninterrupted production process, high-power laser radiation gasification and chemical reaction process, gasification reactor temperature control and cooling process, particle suspension growth control process, dual particle growth furnace parallel process, particle growth furnace temperature control and heat dissipation process, sudden cooling and shaping process, multi-stage rapid cooling process, multi-stage dust collection process, nitrogen circulation process, and full-process monitoring process.

[0036] The whole process is simple, with few steps and easy control and operation. The gasification and chemical reaction, synthetic growth, cooling and collection of materials are completed quickly and continuously in a short time, with short production cycle, high efficiency, low energy consumption, no pollution and small equipment investment, which is very suitable for large-scale production.

[0037] At the same time, by adjusting the process parameters, this process can be applied to the production of a variety of nitride nano-powder materials. It has strong adaptability to raw materials, and both powder and sand can be put into production. There is no need to replace the production line when the raw materials change. Therefore, it can significantly save equipment investment costs and reduce production costs.

[0038] The beneficial effects of the present invention are summarized as follows:

[0039] (1) Simple, efficient and widely applicable process: The present invention proposes a feasible scheme for preparing nitride nano-powder materials by laser gasification and chemical reaction, which utilizes high-power laser, efficient and clean energy. The process is simple, fast and efficient, and does not require complicated equipment and operation. The production line is suitable for a variety of metal or non-metal raw materials and has a wide range of applications.

[0040] (2) Safe and reliable process: The production process is carried out under normal pressure and in a closed nitrogen environment, without the need for complex vacuum or ultra-low pressure and highly closed process equipment. This significantly reduces the complexity of process equipment and the design and manufacturing costs, improves production safety, makes process control operations simple and easy, and ensures safe and reliable equipment operation.

[0041] (3) Controllable particle size: A high-temperature particle growth control process is proposed. By setting the furnace chamber length and adjusting process parameters such as air flow velocity, air flow temperature, and temperature drop gradient, the particle size and distribution range of the micropowder can be precisely controlled, including ultrafine powder or larger particle size powder. This can meet the diverse needs of different fields for nanomaterials.

[0042] (4) High quality of product particle size and uniformity: The suspended particle growth process is adopted, and the crystal nucleus particles are suspended in the high-temperature airflow and further collide and grow naturally. The carbon dioxide low-temperature refrigerant rapid cooling and shaping process is adopted to make the suspended particles quickly condense and shape into spheres or irregular crystals, which significantly improves the product spheroidization rate and crystal quality. Then, through the multi-stage dust collection process, the product can be accurately graded, and the product fineness and uniformity quality can be further improved, thereby effectively improving the product performance.

[0043] (5) High product purity: The production process uses high-purity raw materials, vacuum pretreatment and a closed nitrogen environment at normal pressure. The laser radiation energy used is a non-contact heat source, and no impurities are generated during the production process, ensuring the high purity of the product.

[0044] (6) Continuous batch production: Through the storage tank pre-storage device, continuous feeding device and subsequent continuous process flow, continuous feeding and continuous production are achieved, meeting the needs of batch and large-scale production and realizing industrial production.

[0045] (7) Energy saving and consumption reduction: Through the nitrogen circulation process, the nitrogen in the production process is recycled and reused to reduce emissions, effectively reducing energy consumption and production costs.

[0046] (8) Pollution-free production: No waste gas, waste water or solid waste is discharged during the production process, which does not cause environmental pollution.

[0047] In summary, the present invention can prepare ultrafine, high-purity, uniform-size, high-quality nano-scale nitride micropowder, the production process is simple and easy, the production process is pollution-free, safe and reliable, the production cycle is short, the efficiency is high, the energy consumption is low, the investment is small, the output is high, it can be used for mass industrial production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0049] Figure 1 It is a schematic diagram of the structural principle of the complete set of equipment system of the present invention.

[0050] exist Figure 1 In: 1. High-power laser; 2. Gasification reactor; 3. Gasification platform; 4. Particle growth furnace; 5. Quench cooler; 6. Water-air cooler; 7. Dust collector; 8. Storage tank; 9. Feeding device; 10. Nitrogen generator; 11. Fan; 12. Electric heater; 13. Vacuum unit; 14. Circulation pipeline; 15. Monitoring system. DETAILED DESCRIPTION

[0051] Example 1: Preparation method of nano aluminum nitride powder.

[0052] like Figure 1As shown, the complete set of equipment used in the preparation method includes: a high-power laser 1, a gasification reactor 2, a particle growth furnace 4, a quencher 5, a water-air cooler 6, a dust collector 7, a nitrogen generator 10, a storage tank 8, a vacuum unit 13, and a monitoring system 15. The entire process is completed in a relatively closed airflow channel, starting from the preparation of nitrogen by the nitrogen generator 10, and along the flow direction of nitrogen, the gasification reactor 2, the particle growth furnace 4, the quencher 5, the water-air cooler 6 and the inner cavity of the dust collector 7 are connected in sequence through pipelines to form the entire airflow channel. At the same time, a circulation pipeline 14 is installed at the end of the airflow channel to connect to the outlet of the nitrogen generator 10, and the nitrogen is refluxed for recycling. The storage tank 8 is used to store raw materials and is equipped with a feeding device 9 for pushing the raw materials to the gasification platform 3 in the gasification reactor 2. The outlet of the nitrogen generator 10 is connected to two branch pipes, one of which is connected to the storage tank 8; the other is connected to the fan 11 and the electric heater 12, and then connected to the gasification reactor 2, which is used to provide the gasification reactor with a nitrogen gas flow with controllable flow and temperature. The gasification reactor 2 is equipped with an independent temperature control and cooling device. The particle growth furnace 4 is equipped with a separate temperature control and heat dissipation device and an adjustable damper to adjust and control the air flow temperature and air flow rate; if the product accuracy requires, it is convenient for more refined adjustment, and two sets of particle growth furnaces 4 with the same furnace cavity size can be connected in parallel and connected between the gasification reactor 2 and the quencher 5. The vacuum unit 13 is connected to the storage tank 8 and the air flow channel respectively, and is used to pre-vacuum the storage tank 8 and the air flow channel before the complete set of equipment is put into operation. According to the product accuracy requirements, the dust collector 7 uses a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process composed of these dust collectors. The equipment airflow pipeline is equipped with an automatic pressure relief valve, which will automatically release the pressure when the air pressure in the airflow channel exceeds 120KPa. The monitoring system 15 is equipped with a monitoring platform, an early warning and alarm system, and each equipment monitoring subsystem, which is used to monitor, adjust and control the operating status, operating parameters of each equipment and the process parameters of the airflow in the furnace chamber.

[0053] Material selection: Use high-purity aluminum raw materials in granular or powdered form for later use.

[0054] Process preparation: Load the aluminum raw materials required for 1 to 2 shifts into the storage tank 8 from the feeding port of the storage tank 8, close the feeding port to make the storage tank 8 in a closed state, and push a portion of the aluminum raw materials to the gasification platform 3 in the gasification reactor through the feeding device 9. Start the monitoring system 15 and the vacuum unit 13, and under the action of the vacuum pump, remove the original oxygen and air in the storage tank 8 and the air flow channel, and reduce the vacuum pressure to below 100Pa. After the vacuum is completed, close the vacuum pipeline valve and shut down the vacuum machine 13. Then start the nitrogen generator 10 and the fan 11, fill the storage tank 8 and the air flow channel with nitrogen, so that the pressure of the storage tank 8 and the air flow channel reaches normal pressure, that is, 1 atmosphere.

[0055] Process flow: start the electric heater 12 at the outlet of the nitrogen generator 10, the high-power laser 1, the gasification reactor 2 and its temperature control and cooling device, the particle growth furnace 4 and its temperature control and heat dissipation device, the quencher 5, the water-air cooler 6, the dust collector 7 and other equipment in sequence to put the entire set of equipment into operation. Under the action of the fan 11, the nitrogen circulates in the air flow channel and the circulation pipeline 14, and the nitrogen is supplemented by the nitrogen generator 10. At the same time, the power of the electric heater 12 is adjusted and controlled to heat the nitrogen to above 500°C. In the gasification reactor 2, the laser emitted by the high-power laser 1 directly acts on the raw materials on the gasification platform 3, so that the raw materials are rapidly heated and gasified and react with nitrogen to form aluminum nitride, and then rapidly cooled by the temperature gradient to condense into aluminum nitride crystal nucleus particles, which are suspended in nitrogen. Under the action of airflow, aluminum nitride crystal nucleus particles enter the particle growth furnace 4 with high-temperature airflow. The temperature and velocity of the airflow are adjusted by adjusting the temperature control and heat dissipation device and the adjustable air door of the particle growth furnace 4, so that the airflow temperature at the outlet of the particle growth furnace 4 is not lower than the melting point of aluminum nitride. The aluminum nitride crystal nucleus particles further collide and condense in the high-temperature airflow disturbance to grow particles. After that, they enter the quencher 5 with the airflow. The quencher 5 uses carbon dioxide low-temperature refrigerant. The aluminum nitride particles are rapidly cooled, the temperature drops below its melting point, and they are rapidly solidified and shaped to form solid aluminum nitride powder. Then, they enter the water-air cooler 6 with the airflow, the temperature drops below 160°C, and finally enter the dust collector 7 with the airflow to collect high-purity nano-grade aluminum nitride powder with an average particle size of D50 5-100nm.

[0056] In the above process flow, the melting point of aluminum nitride is 2200°C.

[0057] Example 2: Preparation method of nano titanium nitride powder.

[0058] The complete set of equipment used in this preparation method is the same as that in Example 1.

[0059] Material selection: Use high-purity titanium raw materials in granular or powdered form for future use.

[0060] Process preparation: The titanium raw materials required for 1 to 2 shifts are pre-loaded into the storage tank 8, and the remaining operations are the same as the process preparation in Example 1.

[0061] Process flow: It is similar to the process flow of Example 1, except that the melting point of titanium nitride is 2930°C, the titanium raw material is gasified in the gasification reactor 2 and reacts with nitrogen to synthesize titanium nitride, and then rapidly cooled to form titanium nitride crystal nucleus particles, which grow with the air flow in the particle growth furnace 4, solidify into titanium nitride powder in the quencher 5, and then cool through the water-air cooler 6, and collect through the dust collector 7 to obtain high-purity nano-scale titanium nitride powder with an average particle size of D50 5 to 100 nm.

[0062] Example 3: Preparation method of nano boron nitride powder.

[0063] The complete set of equipment used in this preparation method is the same as that in Example 1.

[0064] Material selection: Use high-purity boron raw materials in granular or powdered form for standby use.

[0065] Process preparation: The boron raw materials required for 1 to 2 shifts are pre-loaded into the storage tank 8, and the remaining operations are the same as the process preparation in Example 1.

[0066] Process flow: The process flow is similar to that of Example 1, except that the melting point of boron nitride is 2700°C, the boron raw material is gasified in the gasification reactor 2 and reacts with nitrogen to synthesize boron nitride, and then rapidly cooled to form boron nitride crystal nucleus particles, which grow with the air flow in the particle growth furnace 4, solidify into boron nitride powder in the quencher 5, and then cool in the water-air cooler 6, and collect in the dust collector 7 to obtain high-purity nano-scale boron nitride powder with an average particle size of D50 5 to 100 nm.

Claims

1. A method for preparing nitride nanopowder, characterized in that: The invention relates to a preparation method of metal nitride and non-metal nitride nano powder; the preparation method is to use high-density energy radiation of laser in a closed nitrogen environment at normal pressure to rapidly gasify the single metal or non-metal raw material and react with nitrogen to generate nitride, and then cool and condense into spherical or irregular crystal nucleus particles, and then produce nano-level powder material through particle growth, rapid cooling and shaping, cooling and collection processes; the preparation method is completed by a set of equipment; The complete set of equipment includes: a high-power laser, a gasification reactor, a particle growth furnace, a quencher, a water-air cooler, a dust collector, a nitrogen generator, a storage tank, a vacuum unit, and a monitoring system; the entire process is completed in a relatively closed airflow channel, starting from the nitrogen generator preparing nitrogen, along the nitrogen flow direction, the gasification reactor, the particle growth furnace, the quencher, the water-air cooler and the inner cavity of the dust collector are connected in sequence through pipelines to form the entire airflow channel; at the same time, a circulation pipeline is installed at the end of the airflow channel and connected to the outlet of the nitrogen generator to reflux the nitrogen for recycling; In the complete set of equipment, the storage tank is used to store metal or non-metal raw materials, and is equipped with a feeding device for pushing the metal or non-metal raw materials to the gasification platform in the gasification reactor; the outlet of the nitrogen generator is connected to two branch pipes, one of which is connected to the storage tank for replenishing nitrogen to the storage tank, and the other is connected to a fan and an electric heater, and then connected to the gasification reactor, for providing a nitrogen gas flow with controllable flow and temperature to the gasification reactor; the gasification reactor is equipped with an independent temperature control and cooling device; the particle growth furnace is equipped with a separate temperature control heat dissipation device and an adjustable damper for adjusting and controlling the gas flow temperature and gas flow rate; the vacuum unit is respectively connected to the storage tank and the gas flow channel, and is used to pre-vacuum the storage tank and the gas flow channel before the complete set of equipment is put into operation; the monitoring system is used to monitor, adjust and control the operating status, operating parameters and process parameters of the gas flow in the furnace cavity of each device throughout the process; The process measures adopted in the process flow include: vacuum pretreatment process, normal pressure, closed nitrogen environment production process, oxygen-free storage and feeding process in storage tanks, nitrogen preheating process, continuous and uninterrupted production process, high-power laser radiation gasification and chemical reaction process, gasification reaction furnace temperature control and cooling process, particle suspension growth control process, particle growth furnace temperature control and heat dissipation process, quenching and shaping process, multi-stage rapid cooling process, multi-stage dust collection process, nitrogen circulation process, and full-process monitoring process; The process specifically comprises the following steps: Step (1): Select a single element metal or single element non-metal material in the form of granules or powder with high purity as a raw material for standby use; Step (2): loading the raw materials required for one to two shifts into the storage tank from the feeding port of the storage tank, closing the feeding port to make the storage tank airtight, and pushing a portion of the raw materials onto the gasification platform in the gasification reactor through the feeding device; Step (3): Start the monitoring system and the vacuum unit, and under the action of the vacuum pump, remove the original oxygen and air in the storage tank and the air flow channel, and reduce the vacuum pressure to below 100Pa; after the vacuuming is completed, close the vacuum pipeline valve and shut down the vacuum unit; then start the nitrogen generator and the blower to fill the storage tank and the air flow channel with nitrogen, so that the pressure of the storage tank and the air flow channel reaches normal pressure, that is, 1 atmosphere; Step (4): sequentially start the high-power laser, the gasification reactor and its temperature control and cooling device, the particle growth furnace and its temperature control and heat dissipation device, the quencher, the water-air cooler, and the dust collector to put the entire set of equipment into operation; under the action of the fan, the nitrogen circulates in the air flow channel and the circulation pipeline, and the nitrogen is supplemented by the nitrogen generator; optionally, for the preparation of nitride nanopowders with a melting point above 1000°C, the electric heater at the outlet of the nitrogen generator can be started at the same time to heat the nitrogen to 500°C to 800°C before entering the gasification reactor; Step (5): In the gasification reaction furnace, the laser light emitted by the high-power laser is directly applied to the raw materials on the gasification platform, and the high-density energy radiation of the laser is used to rapidly heat up the elemental metal or non-metal raw materials, gasify them, and react with nitrogen to form nitrides, which are then rapidly cooled down by the temperature gradient to condense into spherical or irregular shaped nitride crystal nucleus particles, which are suspended in the nitrogen; the nitrogen is also rapidly heated to form a high-temperature airflow; Step (6): under the action of airflow, the crystal nucleus particles of the nitride enter the particle growth furnace along with the high-temperature airflow; the particle growth furnace is equipped with a temperature-controlled heat sink and an adjustable air door for adjusting and controlling the airflow temperature and airflow velocity, so that the airflow temperature at the outlet of the particle growth furnace is not lower than the melting point temperature of the nitride, and the crystal nucleus particles of the nitride further collide and condense in the high-temperature airflow disturbance to grow particles; the size of the growing particles is affected by the cavity length of the particle growth furnace, the airflow temperature, and the airflow velocity of the particle growth furnace. By setting the cavity length of the particle growth furnace, and controlling the airflow temperature and airflow velocity by the temperature-controlled heat sink and the adjustable air door, the collision growth time and particle size of the suspended particles are controlled, thereby achieving accurate particle size classification; Step (7): the grown nitride particles flow rapidly into a quencher along with the air flow, and the quencher uses carbon dioxide as a low-temperature refrigerant; in the low-temperature environment, the nitride particles are rapidly cooled, and the temperature drops below the melting point of the nitride. The rapid temperature change causes the nitride particles to rapidly solidify and form solid micropowders; Step (8): the solid micropowder then enters the water-air cooler along with the air flow. The water-air cooler adopts a multi-stage cooling method of water cooling plus air cooling to reduce the temperature of the solid micropowder to below 160° C. before entering the dust collector. Step (9): Finally, the solid micropowder enters the dust collector along with the airflow and is collected by the dust collector to obtain high-purity nano-scale micropowder; In the above process flow, metal or non-metal raw materials are pre-stored in storage tanks, which are continuously fed to the gasification reactor by a feeding device, and nitrogen is continuously added to the air flow channel in the inner cavity of the equipment by a nitrogen generator. The raw materials are continuously subjected to laser radiation gasification and chemical reaction, condensation growth, rapid cooling and shaping, cooling, and collection. The production process is a continuous and uninterrupted production process.

2. The method for preparing nitride nanopowder according to claim 1, characterized in that: The raw material is any one of a single metal or a single non-metal material, including any one of aluminum, copper, magnesium, nickel, lithium, tungsten, iron, calcium, chromium, zinc, titanium, zirconium, tin, cobalt, hafnium, gallium, strontium, bismuth, vanadium, molybdenum, tantalum, niobium, antimony, germanium, manganese, carbon, silicon, and boron.

3. The method for preparing nitride nanopowder according to claim 1, characterized in that: The particle growth furnace is provided with two sets of particle growth furnaces with the same furnace chamber size connected in parallel and connected between the gasification reaction furnace and the quencher, wherein the furnace chamber size of a single set of particle growth furnaces is designed to meet the production of ultrafine powders, and both are provided with independent temperature control and heat dissipation devices and adjustable air doors; when only one set of particle growth furnaces is opened to participate in production operation, ultrafine powders can be produced; when both sets of particle growth furnaces are opened to participate in production operation at the same time, due to the diversion effect, the air flow velocity in the furnace chamber is reduced, and the collision growth residence time of the suspended particles in the furnace chamber is prolonged, thereby generating micro powders with larger particle sizes to meet the product precision requirements.

4. The method for preparing nitride nanopowder according to claim 1, characterized in that: The average particle size of the nitride nano powder produced by the preparation method is: D50 5-100nm.

5. The method for preparing nitride nanopowder according to claim 1, characterized in that: The dust collector is a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process combining these dust collectors, wherein the electrostatic dust collector uses a single-stage or multi-stage electrostatic dust collector to achieve accurate classification and collection of micro-powder materials.

6. The method for preparing nitride nanopowder according to claim 1, characterized in that: The monitoring system is provided with a monitoring platform, an early warning and alarm system and various equipment monitoring subsystems.

7. The method for preparing nitride nanopowder according to claim 1, characterized in that: The air flow pipeline of the complete set of equipment is equipped with an automatic pressure relief valve, which will automatically relieve pressure when the air pressure in the air flow channel exceeds 120KPa.

8. The method for preparing nitride nanopowder according to claim 1, characterized in that: The furnace chamber material of the gasification reaction furnace and the particle growth furnace is a composite ultra-high temperature ceramic material of zirconium boride and hafnium boride with a refractory temperature of more than 3000°C.